Quick-dry fabric for down jacket lining and preparation method of quick-dry fabric

Through the weaving of modified polyurethane fibers and acetate fibers and the composite technology of electrospinning films modified with sodium alginate and calcium lactate, the problems of the reduction in the quick-drying performance and complex process of existing quick-drying fabrics are solved, and the fabric is lasting It has fast drying and improved antibacterial properties, suitable for use in down jackets.

CN118927734AActive Publication Date: 2024-11-12GAOFAN (ZHEJIANG) INFORMATION TECH CO LTD

Patent Information

Application Number
CN202410998669.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The rapid-drying fabrics have reduced their performance after increasing the number of washes, and the preparation process is complex and difficult to apply on a large scale.

Method used

Modified polyurethane fiber and acetate fiber are woven to obtain a base cloth, and the electrospinned polyvinylidene fluoride film is modified using sodium alginate and calcium lactate to prepare a composite fiber membrane, and the composite fiber membrane is calendered and laminated on the base cloth. The fabric is combined with pickling treatment to improve moisture absorption, quick drying and antibacterial properties.

Benefits of technology

It realizes the long-lasting and excellent wet-guided and fast-drying properties and antibacterial properties of the fabric, simplifies the process flow, and is suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of fabrics, and particularly discloses a quick-dry fabric for down jacket linings and a preparation method thereof.The quick-dry fabric structurally comprises base cloth and a composite fiber membrane composited on one side of the base cloth; the composite fiber membrane is obtained by modifying an electrostatic spinning polyvinylidene fluoride membrane by using sodium alginate and calcium lactate; the base cloth is obtained by weaving modified polyurethane fibers serving as warp yarns and cellulose acetate fibers serving as weft yarns, and the modified polyurethane fibers are obtained by mixing, melting, extruding and spinning raw materials in percentage by mass as follows: 85%-95% of polyurethane slices, 5%-10% of calcium titanate, 0.5%-1% of a surfactant and 0.5%-1% of a dispersing agent. The obtained quick-drying fabric has excellent moisture-conducting quick-drying property and antibacterial property, the process is simple, and the application prospect is good.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention belongs to the technical field of fabrics, and specifically discloses a quick-drying fabric for the lining of down jackets and a preparation method thereof. The structure of the quick-drying fabric includes a base fabric and a composite fiber membrane composited on one side of the base fabric, wherein the composite fiber membrane is obtained by modifying an electrostatically spun polyvinylidene fluoride membrane using sodium alginate and calcium lactate; the base fabric is obtained by weaving a modified polyurethane fiber as a warp yarn and acetate fiber as a weft yarn, and the modified polyurethane fiber is obtained by mixing, melt extruding, and spinning the following raw materials in mass percentage: 85-95% polyurethane slices, 5-10% calcium titanate, 0.5-1% surfactant, and 0.5-1% dispersant. The quick-drying fabric obtained by the invention has excellent moisture conduction and quick-drying properties and antibacterial properties, and has a simple process and good application prospects.

[0002] 1. A quick-drying fabric for the lining of a down jacket, characterized in that the structure of the quick-drying fabric comprises a base fabric and a composite fiber membrane composited on one side of the base fabric, wherein the composite fiber membrane is obtained by modifying an electrostatically spun polyvinylidene fluoride membrane using sodium alginate and calcium lactate;

[0003] The base fabric is obtained by weaving with modified polyurethane fiber as warp yarn and acetate fiber as weft yarn. The modified polyurethane fiber is obtained by mixing, melt extruding and spinning the following raw materials in mass percentage: 85-95% polyurethane chips, 5-10% calcium titanate, 0.5-1% surfactant and 0.5-1% dispersant.

[0004] 2. The quick-drying fabric for the lining of down jackets according to claim 1 is characterized in that the weaving density of the warp is 45-55 threads / cm, the weaving density of the weft is 45-60 threads / cm, and the weaving structure is plain weave.

[0005] 3. The quick-drying fabric for the lining of down jackets according to claim 1 is characterized in that the preparation method of the composite fiber membrane is: firstly dissolve the dried polyvinylidene fluoride powder in a solvent, stir and dissolve to obtain a polyvinylidene fluoride spinning solution, electrospin the polyvinylidene fluoride spinning solution into a fiber membrane, and then soak the fiber membrane with ethanol, immerse it in a sodium alginate solution for 1-5 minutes, and then take it out and immerse it in a calcium lactate solution for 1-5 minutes to obtain the composite fiber membrane.

[0006] 4. The quick-drying fabric for the lining of down jackets according to claim 3 is characterized in that the process parameters of the electrospinning are: the electrospinning voltage is 15-19 kV, the temperature is 20±2°C, the relative humidity is 45±5%, the spinning solution flow rate is 1-3 ml / h, and the distance between the collection roller and the needle is 10-15 cm.

[0007] 5. The quick-drying fabric for down jacket lining according to claim 3, characterized in that the mass fraction of the polyvinylidene fluoride spinning solution is 10-15%, the concentration of the calcium lactate solution is 0.02-0.05 mol / L, and the mass fraction of the sodium alginate solution is 0.2-0.5%.

[0008] 6. A method for preparing the quick-drying fabric for the lining of down jackets as claimed in any one of claims 1 to 5, characterized in that it comprises the following steps:

[0009] (1) preparing modified polyurethane fibers, mixing polyurethane chips, calcium titanate, a surfactant and a dispersant for 10-20 minutes, mixing and granulating through a twin-screw extruder, air-cooling and pelletizing to obtain master batches, and then placing the master batches in a melt spinning machine for spinning to obtain modified polyurethane fibers;

[0010] (2) preparing a base fabric by weaving the modified polyurethane fiber as the warp yarn and the acetate fiber as the weft yarn to obtain the base fabric;

[0011] (3) A composite fiber membrane obtained by modifying the electrospun polyvinylidene fluoride membrane using sodium alginate and calcium lactate;

[0012] (4) The composite fiber membrane is calendered and laminated on one side of the base fabric, and then subjected to a shaping treatment to obtain the quick-drying fabric for the lining of a down jacket.

[0013] 7. The method for preparing quick-drying fabric for down jacket lining according to claim 6 is characterized in that, after step (2), it also includes the steps of washing the base fabric with a heated hydrochloric acid solution having a mass fraction of 20%, and then washing, drying and ironing the base fabric with clean water.

[0014] Quick-drying fabric for down jacket lining and preparation method thereof Technical Field

[0015] The invention belongs to the technical field of fabrics, and in particular relates to a quick-drying fabric for the lining of a down jacket and a preparation method thereof. Background Art

[0016] Quick-drying fabrics have the excellent properties of easy moisture conduction and quick moisture dissipation. When actually worn, they can conduct sweat and moisture from the skin through the inner layer of the fabric to the outer layer. Then the sweat quickly diffuses in the outer layer of the fabric and carries away moisture through convection with the air, keeping the fabric dry and comfortable. For the fabrics lining down jackets, in order to avoid the breeding of bacteria and mites when worn, the fabrics are also required to have moisture conduction and quick-drying properties during the actual production process.

[0017] Regarding the development of quick-drying fabrics, the prior art, such as patent number CN114250541B, discloses a quick-drying fabric, which is immersed in the hydrophilic finishing liquid by innovatively designing the component formula of the hydrophilic finishing liquid. The obtained quick-drying fabric can drain sweat from the body to the surface of the fabric more quickly, and is comfortable to wear. However, the method of immersing the fabric in the hydrophilic finishing liquid cannot guarantee that the fabric has a long-lasting quick-drying performance. As the number of washings increases, its quick-drying performance will decrease accordingly, and the use effect is not good. In addition, the prior art also discloses a process for profiling the fiber cross-section to increase the fiber surface area and thereby improve the moisture conductivity, but due to the complex preparation process, it is difficult to apply on a large scale. Summary of the invention

[0018] In order to solve the above problems, the primary purpose of the present invention is to provide a quick-drying fabric for the lining of a down jacket and a preparation method thereof.

[0019] The specific technical solutions of the present invention include:

[0020] As a first aspect of the present invention, a quick-drying fabric for the lining of a down jacket is provided, wherein the structure of the quick-drying fabric comprises a base fabric and a composite fiber membrane composited on one side of the base fabric, wherein the composite fiber membrane is obtained by modifying an electrostatically spun polyvinylidene fluoride membrane using sodium alginate and calcium lactate;

[0021] The base fabric is obtained by weaving with modified polyurethane fiber as warp yarn and acetate fiber as weft yarn. The modified polyurethane fiber is obtained by mixing, melt extruding and spinning the following raw materials in mass percentage: 85-95% polyurethane chips, 5-10% calcium titanate, 0.5-1% surfactant and 0.5-1% dispersant.

[0022] As a further optimization scheme of the present invention, the weaving density of the warp is 45-55 threads / cm, the weaving density of the weft is 45-60 threads / cm, and the weaving structure is plain weave.

[0023] As a further optimization scheme of the present invention, the preparation method of the composite fiber membrane is: first dissolve the dried polyvinylidene fluoride powder in a solvent, stir and dissolve to obtain a polyvinylidene fluoride spinning solution, electrospin the polyvinylidene fluoride spinning solution into a fiber membrane, and then soak the fiber membrane with ethanol, immerse it in a sodium alginate solution for 1-5 minutes, and then take it out and immerse it in a calcium lactate solution for 1-5 minutes to obtain the composite fiber membrane.

[0024] As a further optimization scheme of the present invention, the process parameters of the electrospinning are as follows: the electrospinning voltage is 15-19 kV, the temperature is 20±2°C, the relative humidity is 45±5%, the spinning solution flow rate is 1-3 ml / h, and the distance between the collection roller and the needle is 10-15 cm.

[0025] As a further optimization scheme of the present invention, the mass fraction of the polyvinylidene fluoride spinning solution is 10-15%, the concentration of the calcium lactate solution is 0.02-0.05 mol / L, and the mass fraction of the sodium alginate solution is 0.2-0.5%.

[0026] As a second aspect of the present invention, there is also provided a method for preparing a quick-drying fabric for the lining of a down jacket as described above, comprising the following steps:

[0027] (1) preparing modified polyurethane fibers, mixing polyurethane chips, calcium titanate, a surfactant and a dispersant for 10-20 minutes, mixing and granulating through a twin-screw extruder, air-cooling and pelletizing to obtain master batches, and then placing the master batches in a melt spinning machine for spinning to obtain modified polyurethane fibers;

[0028] (2) preparing a base fabric by weaving the modified polyurethane fiber as the warp yarn and the acetate fiber as the weft yarn to obtain the base fabric;

[0029] (3) A composite fiber membrane obtained by modifying the electrospun polyvinylidene fluoride membrane using sodium alginate and calcium lactate;

[0030] (4) The composite fiber membrane is calendered and laminated on one side of the base fabric, and then subjected to a shaping treatment to obtain the quick-drying fabric for the lining of a down jacket.

[0031] As a further optimization scheme of the present invention, the step (2) further includes the steps of washing the base fabric with a heated hydrochloric acid solution having a mass fraction of 20%, and then washing, drying and ironing the base fabric with clean water.

[0032] In summary, the beneficial effects of the present invention are:

[0033] (1) The present invention uses calcium titanate to modify polyurethane fiber to obtain modified polyurethane fiber, which is used as warp yarn, and acetate fiber is used as weft yarn to weave a base fabric, and the base fabric is acid-washed to make its surface rough to form pits or hollow structures, thereby enhancing the capillary action on the surface of the base fabric, thereby improving the moisture absorption, quick-drying and antibacterial properties of the overall fabric;

[0034] (2) The present invention obtains a composite fiber membrane by modifying the electrospun polyvinylidene fluoride membrane with sodium alginate and calcium lactate, thereby improving the hydrophilicity of the membrane. After the membrane and the base fabric are composited, there is a difference in hydrophilicity between the two. Water molecules can be quickly conducted from one side of the base fabric, and then evaporate from the base membrane to the outside to complete the quick-drying process, thereby improving the moisture absorption and quick-drying performance of the fabric. DETAILED DESCRIPTION

[0035] The present application is described in further detail below. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technicians in this field can make some non-essential improvements and adjustments to the present application based on the above application content.

[0036] Example 1

[0037] The present embodiment provides a quick-drying fabric for the lining of a down jacket, wherein the structure of the quick-drying fabric includes a base fabric and a composite fiber membrane composited on one side of the base fabric, wherein the composite fiber membrane is obtained by modifying an electrospun polyvinylidene fluoride membrane using sodium alginate and calcium lactate; when the quick-drying fabric is used to prepare a down jacket, the side of the base fabric that is not composited with the composite fiber membrane serves as the skin-friendly side.

[0038] The base fabric is obtained by weaving modified polyurethane fiber as warp yarn and acetate fiber as weft yarn, the weaving density of the warp yarn is 45 yarns / cm, the weaving density of the weft yarn is 45 yarns / cm, and the weaving structure is plain weave. The modified polyurethane fiber is obtained by mixing, melt extruding, and spinning the following raw materials in mass percentage: 93% polyurethane chips, 5% calcium titanate, 1% surfactant, and 1% dispersant.

[0039] The preparation method of the composite fiber membrane is as follows: firstly dissolve the dried polyvinylidene fluoride powder in a mixed solution of N,N-dimethylacetamide and acetone in an equal mass ratio, and obtain a polyvinylidene fluoride spinning solution after stirring and dissolving, wherein the mass fraction of the polyvinylidene fluoride spinning solution is 10%, and the polyvinylidene fluoride spinning solution is electrospinned into a fiber membrane, and the process parameters of the electrospinning are as follows: the electrospinning voltage is 19kV, the temperature is 20°C, the relative humidity is 45%, the spinning solution flow rate is 1ml / h, and the distance between the wire collecting roller and the needle is 15cm. After the obtained fiber membrane is soaked with ethanol, it is immersed in a sodium alginate solution with a mass fraction of 0.5% for 5 minutes, and then it is taken out and immersed in a calcium lactate solution with a concentration of 0.05mol / L for 5 minutes to obtain the composite fiber membrane.

[0040] The preparation method of quick-drying fabric comprises the following steps:

[0041] (1) preparing modified polyurethane fibers, mixing polyurethane chips, calcium titanate, a surfactant (in this embodiment, sodium dodecylbenzene sulfonate) and a dispersant (in this embodiment, a dispersant NNO) for 10 minutes, mixing and granulating through a twin-screw extruder, air-cooling and pelletizing to obtain master batches, and then placing the master batches in a melt spinning machine for spinning to obtain modified polyurethane fibers. The operating temperature of the melt spinning machine from the feed port to the spinneret die can be conventionally adjusted in the polyurethane fiber production process according to the prior art mastered by those skilled in the art, and is not limited here;

[0042] (2) preparing a base fabric by weaving the modified polyurethane fiber as the warp yarn and the acetate fiber as the weft yarn to obtain the base fabric;

[0043] (3) using a heated 20% hydrochloric acid solution to clean the base fabric, and then washing, drying, and ironing the base fabric with clean water for later use;

[0044] (4) A composite fiber membrane obtained by modifying the electrospun polyvinylidene fluoride membrane using sodium alginate and calcium lactate;

[0045] (5) The composite fiber membrane is calendered and bonded to one side of the base fabric, and then subjected to a shaping treatment. Here, the process of calendering and bonding the membrane and the base fabric is an existing technology mastered by technicians in this field and is not limited here. The quick-drying fabric for the lining of down jackets can be obtained.

[0046] Example 2

[0047] The present embodiment provides a quick-drying fabric for the lining of a down jacket, wherein the structure of the quick-drying fabric includes a base fabric and a composite fiber membrane composited on one side of the base fabric, wherein the composite fiber membrane is obtained by modifying an electrospun polyvinylidene fluoride membrane using sodium alginate and calcium lactate; when the quick-drying fabric is used to prepare a down jacket, the side of the base fabric that is not composited with the composite fiber membrane serves as the skin-friendly side.

[0048] The base fabric is obtained by weaving modified polyurethane fiber as warp yarn and acetate fiber as weft yarn, the weaving density of the warp yarn is 55 yarns / cm, the weaving density of the weft yarn is 60 yarns / cm, and the weaving structure is plain weave. The modified polyurethane fiber is obtained by mixing, melt extruding, and spinning the following raw materials in mass percentage: 88% polyurethane chips, 10% calcium titanate, 1% surfactant, and 1% dispersant.

[0049] The preparation method of the composite fiber membrane is as follows: firstly, the dried polyvinylidene fluoride powder is dissolved in a mixed solution of N,N-dimethylacetamide and acetone in an equal mass ratio, and the polyvinylidene fluoride spinning solution is obtained after stirring and dissolving, wherein the mass fraction of the polyvinylidene fluoride spinning solution is 15%, and the polyvinylidene fluoride spinning solution is electrospinned into a fiber membrane, and the process parameters of the electrospinning are the same as those in Example 1. After the obtained fiber membrane is soaked with ethanol, it is immersed in a sodium alginate solution with a mass fraction of 0.5% for 5 minutes, and then it is taken out and immersed in a calcium lactate solution with a concentration of 0.05 mol / L for 5 minutes to obtain the composite fiber membrane.

[0050] The preparation method of the quick-drying fabric is the same as that of Example 1.

[0051] Example 3

[0052] The present embodiment provides a quick-drying fabric for the lining of a down jacket, wherein the structure of the quick-drying fabric includes a base fabric and a composite fiber membrane composited on one side of the base fabric, wherein the composite fiber membrane is obtained by modifying an electrospun polyvinylidene fluoride membrane using sodium alginate and calcium lactate; when the quick-drying fabric is used to prepare a down jacket, the side of the base fabric that is not composited with the composite fiber membrane serves as the skin-friendly side.

[0053] The base fabric is obtained by weaving modified polyurethane fiber as warp yarn and acetate fiber as weft yarn, the weaving density of the warp yarn is 45 yarns / cm, the weaving density of the weft yarn is 45 yarns / cm, and the weaving structure is plain weave. The modified polyurethane fiber is obtained by mixing, melt extruding, and spinning the following raw materials in mass percentage: 94% polyurethane chips, 5% calcium titanate, 0.5% surfactant, and 0.5% dispersant.

[0054] The preparation method of the composite fiber membrane is as follows: firstly, the dried polyvinylidene fluoride powder is dissolved in a mixed solution of N,N-dimethylacetamide and acetone in an equal mass ratio, and the polyvinylidene fluoride spinning solution is obtained after stirring and dissolving, wherein the mass fraction of the polyvinylidene fluoride spinning solution is 15%, and the polyvinylidene fluoride spinning solution is electrospinned into a fiber membrane, and the process parameters of the electrospinning are the same as those in Example 1. After the obtained fiber membrane is soaked with ethanol, it is immersed in a sodium alginate solution with a mass fraction of 0.2% for 5 minutes, and then it is taken out and immersed in a calcium lactate solution with a concentration of 0.02 mol / L for 5 minutes to obtain the composite fiber membrane.

[0055] The preparation method of the quick-drying fabric is the same as that of Example 1.

[0056] Comparative Example 1

[0057] This comparative example provides a quick-drying fabric for the lining of a down jacket. The structure of the quick-drying fabric includes a base fabric and a composite fiber membrane composited on one side of the base fabric. The composite fiber membrane is obtained by modifying an electrostatically spun polyvinylidene fluoride membrane using sodium alginate and calcium lactate.

[0058] The base fabric is obtained by weaving polyurethane fiber as warp yarn and acetate fiber as weft yarn, the weaving density of the warp yarn is 45 yarns / cm, the weaving density of the weft yarn is 45 yarns / cm, and the weaving structure is plain weave. The polyurethane fiber is obtained by mixing, melt extruding, and spinning the following raw materials in mass percentage: 99% polyurethane chips, 0.5% surfactant, and 0.5% dispersant.

[0059] The preparation method of the quick-drying fabric is the same as that of Example 1.

[0060] Comparative Example 2

[0061] This comparative example provides a quick-drying fabric for the lining of a down jacket, wherein the structure of the quick-drying fabric comprises a base fabric and a composite fiber membrane composited on one side of the base fabric, wherein the composite fiber membrane is an electrospun polyvinylidene fluoride membrane;

[0062] The preparation method of electrospun polyvinylidene fluoride membrane is as follows: firstly, the dried polyvinylidene fluoride powder is dissolved in a mixed solution of N,N-dimethylacetamide and acetone in an equal mass ratio, and the polyvinylidene fluoride spinning solution is obtained after stirring and dissolving, wherein the mass fraction of the polyvinylidene fluoride spinning solution is 10%, and the polyvinylidene fluoride spinning solution is formed into a fiber membrane by electrospinning, and the process parameters of the electrospinning are as follows: the electrospinning voltage is 19 kV, the temperature is 20°C, the relative humidity is 45%, the spinning solution flow rate is 1 ml / h, and the distance between the collecting roller and the needle is 15 cm.

[0063] The base fabric is obtained by weaving modified polyurethane fiber as warp yarn and acetate fiber as weft yarn, the weaving density of the warp yarn is 45 yarns / cm, the weaving density of the weft yarn is 45 yarns / cm, and the weaving structure is plain weave. The modified polyurethane fiber is obtained by mixing, melt extruding, and spinning the following raw materials in mass percentage: 93% polyurethane chips, 5% calcium titanate, 1% surfactant, and 1% dispersant.

[0064] The preparation method of the quick-drying fabric is the same as that of Example 1.

[0065] Verification test

[0066] 1. The quick-drying fabrics prepared in Examples 1-3 and Comparative Examples 1-2 were used as samples to determine the antibacterial rate according to FZ / T 73023-2006 "Standard for Antibacterial Knitwear", and the moisture absorption and quick-drying performance was determined according to GB T 21655.1-2008 "Evaluation of Moisture Absorption and Quick-drying Properties of Textiles". The results are shown in Table 1.

[0067] Table 1. Test results statistics

[0068]

[0069] It can be seen from Table 1 that the fabrics prepared in Examples 1-3 are better than those in Comparative Examples 1-2 in terms of moisture absorption and quick-drying performance and antibacterial performance. Specifically, the difference between Comparative Example 1 and Example 1 is that the warp yarn of the base fabric in Comparative Example 1 uses unmodified polyurethane fibers. From the result data, the moisture absorption and quick-drying performance of Comparative Example 1 is lower than that of Example 1, but the antibacterial property is significantly lower than that of Example 1. It can be seen that the use of modified polyurethane fibers has a positive effect on improving the antibacterial property of the fabric.

[0070] The difference between Comparative Example 2 and Example 1 is that the composite fiber membrane used in Comparative Example 2 is an unmodified electrospun polyvinylidene fluoride membrane. From the result data, the moisture absorption and quick-drying performance and antibacterial properties of Comparative Example 2 are significantly lower than those of Example 1. It can be seen that the modification of the electrospun polyvinylidene fluoride membrane has a positive effect on improving the moisture absorption and quick-drying properties and antibacterial properties of the fabric.

[0071] 2. To further study the effect of modified polyurethane fiber on the performance of base fabric, the following comparative examples were set:

[0072] Comparative Example 3

[0073] The only difference between this comparative example and Example 1 is that the modified polyurethane fiber is obtained by mixing, melt extruding and spinning the following raw materials in percentage by mass: 93% polyurethane chips, 5% calcium carbonate, 1% surfactant (sodium dodecylbenzene sulfonate) and 1% dispersant (dispersant NNO).

[0074] Comparative Example 4

[0075] The only difference between this comparative example and Example 1 is that the modified polyurethane fiber is obtained by mixing, melt extruding and spinning the following raw materials in percentage by mass: 93% polyurethane chips, 5% calcium silicate, 1% surfactant (sodium dodecylbenzene sulfonate) and 1% dispersant (dispersant NNO).

[0076] Comparative Example 5

[0077] The only difference between this comparative example and Example 1 is that in the method for preparing the quick-drying fabric, step (3) is not performed.

[0078] The quick-drying fabrics prepared in Comparative Examples 3-5 were used as samples to determine the antibacterial rate according to FZ / T 73023-2006 "Standard for Antibacterial Knitwear", and the moisture absorption and quick-drying performance was determined according to GB T 21655.1-2008 "Evaluation of Moisture Absorption and Quick-drying Properties of Textiles". The results were compared with those of Example 1. The results are shown in Table 2.

[0079] Table 2. Test results statistics

[0080]

[0081] It can be seen from Table 2 that the moisture absorption, quick drying and antibacterial properties of the fabric prepared in Example 1 are better than those of Comparative Examples 3-4. The difference between the three lies in the different modified components. Example 1 uses calcium titanate, and Comparative Examples 3-4 use calcium carbonate and calcium silicate respectively. From the data comparison, it can be seen that calcium titanate and calcium carbonate have the same effect on improving the moisture absorption and quick drying of the fabric, but calcium titanate is better than calcium titanate in improving the antibacterial property of the fabric, while calcium silicate is not as good as Example 1 in improving the moisture absorption, quick drying and antibacterial properties of the fabric.

[0082] In addition, the difference between Comparative Example 5 and Example 1 is that the pickling step is omitted when preparing the fabric in Comparative Example 5. From the data comparison, it can be seen that Example 1 performs the pickling step, and the moisture absorption and quick-drying properties of the fabric are improved to a certain extent. This is because when the base fabric is cleaned with a heated hydrochloric acid solution, the hydrochloric acid acts on the surface of the base fabric and the calcium titanate component in the modified polyurethane fiber, causing a certain amount of dissolution of the calcium titanate. At this time, a certain amount of void structure is correspondingly generated on the surface of the base fabric, which strengthens its capillary action and enhances its own moisture absorption and dehumidification properties.

[0083] 3. The influence of composite fiber membrane on fabric performance will be further explored, and the following comparative examples will be set:

[0084] Comparative Example 6

[0085] The only difference between this comparative example and Example 1 is that the composite fiber membrane is obtained by modifying the electrospun polyvinylidene fluoride membrane using sodium alginate and calcium chloride, and the preparation method of the composite fiber membrane is the same as that of Example 1.

[0086] Comparative Example 7

[0087] The only difference between this comparative example and Example 1 is that the composite fiber membrane is obtained by modifying the electrospun polyvinylidene fluoride membrane with sodium alginate, and the preparation method of the composite fiber membrane is as follows: firstly dissolve the dried polyvinylidene fluoride powder in a mixed solution of equal mass ratio of N,N-dimethylacetamide and acetone, and obtain the polyvinylidene fluoride spinning solution after stirring and dissolving, the mass fraction of the polyvinylidene fluoride spinning solution is 10%, and the polyvinylidene fluoride spinning solution is electrospinned into a fiber membrane, and the process parameters of the electrospinning are as follows: the electrospinning voltage is 19 kV, the temperature is 20°C, the relative humidity is 45%, the spinning solution flow rate is 1 ml / h, the distance between the collecting roller and the needle is 15 cm, and the obtained fiber membrane is soaked with ethanol, and then immersed in a sodium alginate solution with a mass fraction of 0.5% for 10 minutes to obtain the composite fiber membrane.

[0088] The quick-drying fabrics prepared in Comparative Examples 6-7 were used as samples to determine the antibacterial rate according to FZ / T 73023-2006 "Standard for Antibacterial Knitwear", and the moisture absorption and quick-drying performance was determined according to GB T 21655.1-2008 "Evaluation of Moisture Absorption and Quick-drying Properties of Textiles". The results were compared with those of Example 1. The results are shown in Table 3.

[0089] Table 3. Test results statistics

[0090]

[0091] It can be seen from Table 3 that the moisture absorption, quick-drying and antibacterial properties of the fabric prepared in Example 1 are better than those of Comparative Examples 6-7. The difference between the three lies in the different modified components added in the preparation of the composite fiber membrane. Example 1 uses sodium alginate and calcium lactate, Comparative Example 6 uses sodium alginate and calcium chloride respectively, and Comparative Example 7 uses only sodium alginate. From the data comparison, it can be seen that the fabric of Example 1 has better moisture absorption, quick-drying and antibacterial properties. The reason is that the polytetrafluoroethylene membrane is modified by sodium alginate and calcium lactate so that calcium alginate is deposited on the surface of the membrane, so that the hydrophilicity of the membrane is improved, and the hydrophilicity of the membrane and the base fabric form a difference, and water molecules can be quickly conducted from one side of the base fabric. The quick-drying process is then completed by evaporation of the base film to the outside, so that the moisture absorption and quick-drying performance of the fabric is improved. To verify this conclusion, the composite fiber membranes obtained in Example 1 and Comparative Examples 6-7 are subsequently tested for the contact angle of the membrane surface at room temperature using a contact angle meter. The membrane is fixed on a glass slide, 3 μL of liquid is dripped into it, and the change in contact angle during the entire time (10 min) is recorded with a camera. Each membrane sample is measured 3 times to minimize the error. Finally, it is concluded that the contact angle of the composite fiber membrane obtained in Example 1 is 103°, which is a certain degree lower than 125° and 137° of Comparative Examples 6-7. The hydrophilicity of the composite fiber membrane obtained in Example 1 is better than that of Comparative Examples 6-7.

[0092] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A quick-drying fabric for the lining of a down jacket, characterized in that: The structure of the quick-drying fabric includes a base fabric and a composite fiber membrane composited on one side of the base fabric, wherein the composite fiber membrane is obtained by modifying an electrostatically spun polyvinylidene fluoride membrane using sodium alginate and calcium lactate; The base fabric is obtained by weaving with modified polyurethane fiber as warp yarn and acetate fiber as weft yarn. The modified polyurethane fiber is obtained by mixing, melt extruding and spinning the following raw materials in mass percentage: 85-95% polyurethane chips, 5-10% calcium titanate, 0.5-1% surfactant and 0.5-1% dispersant.

2. The quick-drying fabric for the lining of down jackets according to claim 1, characterized in that: The weaving density of the warp is 45-55 threads / cm, the weaving density of the weft is 45-60 threads / cm, and the weaving structure is plain weave.

3. The quick-drying fabric for the lining of down jackets according to claim 1, characterized in that: The preparation method of the composite fiber membrane is as follows: firstly dissolve the dried polyvinylidene fluoride powder in a solvent, stir and dissolve to obtain a polyvinylidene fluoride spinning solution, electrospin the polyvinylidene fluoride spinning solution into a fiber membrane, then soak the fiber membrane with ethanol, immerse it in a sodium alginate solution for 1-5 minutes, then take it out and immerse it in a calcium lactate solution for 1-5 minutes to obtain the composite fiber membrane.

4. The quick-drying fabric for the lining of down jackets according to claim 3, characterized in that: The process parameters of the electrospinning are as follows: the electrospinning voltage is 15-19 kV, the temperature is 20±2° C., the relative humidity is 45±5%, the spinning solution flow rate is 1-3 ml / h, and the distance between the collection drum and the needle is 10-15 cm.

5. The quick-drying fabric for the lining of down jackets according to claim 3, characterized in that: The mass fraction of the polyvinylidene fluoride spinning solution is 10-15%, the concentration of the calcium lactate solution is 0.02-0.05 mol / L, and the mass fraction of the sodium alginate solution is 0.2-0.5%.

6. A method for preparing the quick-drying fabric for the lining of down jackets as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: (1) preparing modified polyurethane fibers, mixing polyurethane chips, calcium titanate, a surfactant and a dispersant for 10-20 minutes, mixing and granulating through a twin-screw extruder, air-cooling and pelletizing to obtain master batches, and then placing the master batches in a melt spinning machine for spinning to obtain modified polyurethane fibers; (2) preparing a base fabric by weaving the modified polyurethane fiber as the warp yarn and the acetate fiber as the weft yarn to obtain the base fabric; (3) A composite fiber membrane obtained by modifying the electrospun polyvinylidene fluoride membrane using sodium alginate and calcium lactate; (4) The composite fiber membrane is calendered and laminated on one side of the base fabric, and then subjected to a shaping treatment to obtain the quick-drying fabric for the lining of a down jacket.

7. The method for preparing the quick-drying fabric for the lining of down jackets according to claim 6, characterized in that: The step (2) also includes the steps of washing the base fabric with a heated hydrochloric acid solution having a mass fraction of 20%, and then washing, drying and ironing the base fabric with clean water.

Citation Information

Patent Citations

  • Nanometer fiber-reinforced hydrogel filter membrane and preparation method thereof

    CN106310957A

  • Clothing material, and production technology thereof

    CN109421355A

  • Special quick-drying fabric for clothing and processing technology thereof

    CN112477330A

  • Processing technology of quick-dry fabric special for clothes

    CN114622408A

Cited By

  • Sweat-absorbing quick-drying fabric and preparation process thereof

    CN119704832A