Resource recycling method for phosphoric acid in phosphorus-sulfur mixed acid

By using hydrated lime and potassium hydroxide to treat phosphosulfur mixed acid, control pH and temperature, and successfully separate and recover sulfate and phosphate, the problems of resource waste and environmental pollution in the existing technology are solved, and efficient utilization of phosphate resources and Economic benefits.

CN118929594APending Publication Date: 2024-11-12WUXI ZHONGTIAN SOLID WASTE DISPOSAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410984313.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively separate sulfate and phosphate in the phosphorus-sulfur mixed acid, and the desulfurizer used is toxic and difficult to filtration, resulting in waste of phosphoric acid resources and environmental pollution.

Method used

Ripped lime is used as a desulfurizer to remove sulfate and avoid phosphate loss by controlling the pH value, temperature and mixing. Potassium hydroxide is used to adjust the pH value and distillate it to extract potassium dihydrogen phosphate.

Benefits of technology

The effective recycling of sulfate and efficient resource utilization of phosphate are achieved, the impact of toxic desulfurizers on the environment is reduced, and economic benefits and resource utilization are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956952630000091
    Figure BDA0004956952630000091
  • Figure BDA0004956952630000101
    Figure BDA0004956952630000101
  • Figure BDA0004956952630000111
    Figure BDA0004956952630000111
Patent Text Reader

Abstract

The invention relates to a method for recycling phosphoric acid in phosphorus-sulfur mixed acid, which comprises the following steps: (1) mixing a phosphorus-sulfur mixed acid solution and slaked lime, and then carrying out solid-liquid separation to obtain filtrate and filter residue containing calcium sulfate dihydrate; (2) mixing the filtrate obtained in the step (1) with potassium hydroxide to adjust the pH value to obtain a potassium-containing solution; and (3) distilling the potassium-containing solution obtained in the step (2), adding phosphoric acid into the distilled mother liquor obtained by distillation to adjust the pH value, and then sequentially cooling and carrying out solid-liquid separation to obtain a monopotassium phosphate product. According to the method provided by the invention, sulfate radicals can be effectively separated from the mixed acid solution, the loss of phosphate radicals is reduced, the resource utilization of phosphoric acid in the phosphorus-sulfur mixed acid is realized, the influence of a toxic desulfurizer on the environment is avoided, and the economic benefit is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste liquid treatment, and in particular to a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid. Background Art

[0002] In the semiconductor industry or metal processing industry, it is often necessary to prepare a mixed acid solution of phosphoric acid and sulfuric acid for acid cleaning, which generates a large amount of phosphorus-sulfur mixed acid waste liquid. Phosphorus is a limited resource that cannot be manufactured or synthesized. If these waste liquids are directly disposed of, it will not only waste resources, but also pollute the environment.

[0003] Sulfuric acid and phosphoric acid are both inorganic acids with similar boiling points, which makes it difficult to effectively separate them by distillation alone. In the existing phosphate rock desulfurization technology, desulfurizers such as barium carbonate and calcium carbonate are commonly used. Although these desulfurizers can remove sulfate components to a certain extent, they are also accompanied by partial loss of phosphoric acid. In addition, barium carbonate itself is toxic and difficult to filter during the treatment process.

[0004] For example, CN114195178A discloses a method for resource utilization of waste sulfuric acid containing phosphoric acid, including: preparing waste sulfuric acid containing phosphoric acid as a target, detecting the phosphate content and sulfate content therein; taking barium carbonate in the amount of substances such as sulfate in the target, adding an acidic solution, and stirring thoroughly to make barium carbonate slurry No. 1; taking barium carbonate in the amount of substances such as phosphate in the target, adding an acidic solution, and stirring thoroughly to make barium carbonate slurry No. 2; first slowly adding barium carbonate slurry No. 1 to the target to remove sulfate, and then slowly adding barium carbonate slurry No. 2 to the filtrate to react, controlling the system pH at 6.5-7.5, and removing phosphate. Although the above method can achieve the separation of barium phosphate and barium sulfate, barium carbonate is toxic, and the precipitated particles are fine, making filtration difficult.

[0005] Therefore, how to effectively separate sulfate and phosphate in phosphorus-sulfur mixed acid and avoid the loss of phosphate to maximize resource utilization is a technical problem that needs to be solved in the current field. Summary of the invention

[0006] In view of the above problems, the purpose of the present invention is to provide a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid. Compared with the prior art, the method provided by the present invention can effectively separate sulfate from the mixed acid solution and significantly reduce the loss of phosphate, thereby realizing the resource utilization of phosphoric acid in phosphorus-sulfur mixed acid, avoiding the impact of toxic desulfurizers on the environment, and significantly improving economic benefits.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] The present invention provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid, the method comprising the following steps:

[0009] (1) mixing a phosphorus-sulfur mixed acid solution and slaked lime, and then performing solid-liquid separation to obtain a filtrate and a filter residue containing calcium sulfate dihydrate;

[0010] (2) mixing the filtrate obtained in step (1) with potassium hydroxide to adjust the pH value to obtain a potassium-containing solution;

[0011] (3) distilling the potassium-containing solution obtained in step (2), adding phosphoric acid to the distillation mother liquor obtained by the distillation to adjust the pH value, and then cooling and solid-liquid separation are performed in sequence to obtain a potassium dihydrogen phosphate product.

[0012] In the method provided by the present invention, slaked lime is used as a desulfurizing agent, and desulfurization is first performed by mixing slaked lime with a phosphorus-sulfur mixed acid solution. During the desulfurization process, the mixed pH value, temperature, and mixing method are strictly controlled to effectively remove sulfate in the phosphorus-sulfur mixed acid solution and avoid the loss of phosphate; then the phosphate in the filtrate is used as a resource, mainly including first using potassium hydroxide to adjust the pH value, introducing potassium ions into the filtrate, then removing excess water by distillation, and adjusting the pH value by adding phosphoric acid to promote the precipitation of potassium dihydrogen phosphate, and then successively cooling and solid-liquid separation to obtain a potassium dihydrogen phosphate product. It can be seen that the method provided by the present invention recovers sulfate in the form of calcium sulfate, prepares potassium dihydrogen phosphate products from phosphate, realizes maximum resource utilization and significant economic benefits, and has great potential in environmental protection and resource utilization.

[0013] Preferably, the mass ratio of phosphate to sulfate in the phosphorus-sulfur mixed acid solution in step (1) is greater than 3, for example, it can be 4, 5, 6, 7 or 8, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0014] In the present invention, the phosphorus-sulfur mixed acid solution is generally derived from a phosphoric acid and sulfuric acid mixed acid solution used for cleaning in the semiconductor industry or the metal processing industry, wherein the concentration of phosphate is 900-2000 g / L, the concentration of sulfate is 150-700 g / L, and the impurity ions include fluoride ions, nitrate ions, etc., and the concentration is generally 50-200 g / L. The phosphorus-sulfur mixed acid solution of the present invention is a phosphorus-sulfur mixed acid solution after the impurity ions such as fluoride ions and nitrate ions are removed in advance by distillation.

[0015] In the present invention, the mass ratio of phosphate to sulfate in the phosphorus-sulfur mixed acid solution is preferably controlled to be greater than 3 because when the mass ratio of phosphate to sulfate is ≤3, the proportion of sulfate is too high, and a large amount of lime is required for removal, resulting in poor desulfurization efficiency. The pH value of the solution may even increase due to a large amount of lime, thereby causing the loss of phosphate.

[0016] Preferably, the mixing in step (1) is carried out under the condition of a pH value of less than 1.5, for example, it can be 1.4, 1.2, 1, 0.8, 0.6, 0.4, 0.2 or 0, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0017] It should be noted that, under normal circumstances, the Ksp of calcium phosphate is much smaller than the Ksp of calcium sulfate, so calcium phosphate in the solution will generally precipitate out first, which will lead to the loss of phosphate. In the present invention, by controlling the mixing in step (1) to be carried out under strong acidic conditions, preferably controlling the mixing to be carried out under the condition of pH value <1.5, the solubility of calcium sulfate can be relatively high, so that the sulfate and calcium ions in slaked lime (calcium hydroxide) can more easily meet in water and undergo a neutralization reaction, on the contrary, the solubility of calcium phosphate is lowered, the frequency of collision between phosphate ions and calcium ions in slaked lime (calcium hydroxide) is reduced, resulting in a slower rate of neutralization reaction, that is, the present invention controls the pH value during the mixing process, so that the sulfate is removed in the form of calcium sulfate to the maximum extent, and the phosphate is retained to the maximum extent, which is conducive to the subsequent realization of phosphate resource utilization to prepare potassium dihydrogen phosphate.

[0018] Preferably, the mixing temperature in step (1) is controlled to be 20-50°C, for example, it can be 20°C, 22°C, 24°C, 26°C, 28°C, 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, 42°C, 44°C, 46°C, 48°C or 50°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] In the present invention, the reaction of slaked lime and sulfuric acid is mainly carried out in the mixing of step (1), and heat is released during the reaction. When the temperature is too high, the solubility of calcium hydroxide is easily reduced, and the generated calcium sulfate is mainly precipitated from the solution in the form of calcium sulfate dihydrate, so when the temperature is too high, the material is viscous and difficult to stir. The present invention can effectively remove sulfate ions in the mixed acid and reduce the loss of phosphate ions by preferably controlling the temperature of the mixing of step (1) within a specific range, which is conducive to improving the purity of the subsequent potassium dihydrogen phosphate.

[0020] In the present invention, the method of solid-liquid separation is not particularly limited, and any method commonly used for solid-liquid separation in the art may be used, such as filtration or centrifugation.

[0021] Preferably, stirring is performed during the mixing process in step (1).

[0022] Preferably, the stirring time is 4-6 h, for example, 4 h, 4.2 h, 4.4 h, 4.6 h, 4.8 h, 5 h, 5.2 h, 5.4 h, 5.6 h, 5.8 h or 6 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the mixing in step (1) controls the Ca(OH)2 in the slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution. 2- The molar ratio of is 1:(1.25-1.5), for example, it can be 1:1.25, 1:1.3, 1:1.35, 1:1.4, 1:1.45 or 1:1.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] In the present invention, it is preferred to control the Ca(OH)2 in the slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution. 2- The molar ratio of slaked lime to slaked lime can avoid the situation where, when excessive slaked lime is added, more sulfate ions can be removed, but more calcium ions remain, resulting in the conversion into calcium phosphate in the subsequent cooling step, thereby causing the loss of phosphate ions; at the same time, it can also avoid the situation where, when too little slaked lime is added, sulfate ions in the mixed acid cannot be effectively removed, thereby causing the separation effect to deteriorate.

[0025] Preferably, the mixing in step (1) comprises adding slaked lime into the phosphorus-sulfuric acid solution in batches.

[0026] Preferably, the mass of slaked lime added in each batch accounts for 5-10% of the total mass of slaked lime, for example, it can be 5%, 6%, 7%, 8%, 9% or 10%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the time interval for adding each batch is 5-15 min, for example, it can be 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min or 15 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] In the present invention, it is preferred to control the slaked lime to be added to the mixed acid solution in batches during the mixing in step (1), and by preferably controlling the percentage of the mass of slaked lime added in each batch to the total mass of slaked lime, the time interval for adding each batch, and other conditions, the mixing process can be further controlled to adapt to the viscosity and temperature changes of the reactants, avoid heat release caused by too fast reaction and avoid local solution viscosity, promote the full reaction of sulfate, avoid the loss of phosphate, and further ensure the purity of the subsequent potassium dihydrogen phosphate.

[0029] Preferably, the calcium sulfate dihydrate-containing filter residue in step (1) is washed to obtain a washed liquid and calcium sulfate dihydrate.

[0030] Preferably, the filtrate is mixed with the washed solution, and then potassium hydroxide is added to adjust the pH value.

[0031] In the present invention, the post-cleaning liquid is a dilute phosphoric acid solution, and mixing the post-cleaning liquid with the filtrate can further reduce the loss of phosphate radicals and improve the recovery rate of phosphate radicals.

[0032] Preferably, the mass ratio of phosphate to sulfate in the solution obtained by mixing the filtrate and the cleaned liquid is (28-35):1, for example, it can be 28:1, 28.5:1, 29:1, 29.5:1, 30:1, 30.5:1, 31:1, 31.5:1, 32:1, 32.5:1, 33:1, 33.5:1, 34:1, 34.5:1 or 35:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the washing liquid used in the washing in step (1) comprises water.

[0034] Preferably, the water temperature used for cleaning is 50-60°C, for example, it can be 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] In the present invention, by preferably controlling the water temperature used for the cleaning within a specific range, it is beneficial to promote the softening of the filter residue and prevent the over-hard filter residue from affecting the recovery of phosphate in the filter residue.

[0036] Preferably, the endpoint pH value of the pH adjustment in step (2) is 6-7, for example, 6, 6.2, 6.4, 6.6, 6.8 or 7, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0037] Preferably, the specific gravity of the solution distilled in step (3) is 1.5-1.7, for example, it can be 1.5, 1.52, 1.54, 1.56, 1.58, 1.6, 1.62, 1.64, 1.66, 1.68 or 1.7, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0038] In the present invention, by preferably controlling the specific gravity of the solution within a specific range, the water content can be further reduced, which is beneficial to the subsequent precipitation of potassium dihydrogen phosphate.

[0039] Preferably, the endpoint pH value of the pH adjustment is 4.2-4.5, for example, it can be 4.2, 4.22, 4.24, 4.26, 4.28, 4.3, 4.32, 4.36, 4.38, 4.4, 4.42, 4.44, 4.46, 4.48 or 4.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] In the present invention, by preferably controlling the end point pH range of the pH value correction, the crystallization of potassium dihydrogen phosphate can be further promoted.

[0041] Preferably, the cooling to the terminal temperature is 35-40°C, for example, 35°C, 36°C, 37°C, 38°C, 39°C or 40°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] In the present invention, the filtrate obtained after the solid-liquid separation in step (3) is pretreated and then used for distillation to prepare potassium dihydrogen phosphate or used as dilution water for high-concentration phosphorus-sulfuric acid.

[0043] As a preferred technical solution of the present invention, the method comprises the following steps:

[0044] (1) mixing a phosphorus-sulfuric acid solution and slaked lime at a pH value of less than 1.5 and a temperature of 20-50° C., wherein the mixing comprises adding slaked lime to the phosphorus-sulfuric acid solution in a manner such that the mass of slaked lime added in each batch accounts for 5-10% of the total mass of slaked lime and the time interval between each batch is 5-15 minutes, and the mixing is controlled to reduce the Ca(OH)2 in the slaked lime to SO4 in the phosphorus-sulfuric acid solution. 2- The molar ratio of the mixture is 1:(1.25-1.5), the mixing process is stirred for 4-6 hours, and then the solid-liquid separation is performed to obtain a filtrate and a filter residue containing calcium sulfate dihydrate, the filter residue containing calcium sulfate dihydrate is washed to obtain a washed liquid and calcium sulfate dihydrate, and the water temperature used for the washing is 50-60°C;

[0045] (2) mixing the cleaned liquid and the filtrate obtained in step (1), wherein the mass ratio of phosphate to sulfate in the obtained solution is (28-35):1, and then adding potassium hydroxide to adjust the pH value to an end point pH value of 6-7 to obtain a potassium-containing solution;

[0046] (3) distilling the potassium-containing solution obtained in step (2) until the solution has a specific gravity of 1.5-1.7, adding phosphoric acid to the mother liquor obtained by distillation to adjust the pH value to an end point pH value of 4.2-4.5, then cooling to an end point temperature of 35-40° C., and then solid-liquid separation to obtain a potassium dihydrogen phosphate product.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] (1) In the method provided by the present invention, by using slaked lime as a desulfurizing agent and strictly controlling the pH value, temperature, and addition method during the slaked lime reaction process, the sulfate in the phosphorus-sulfur mixed acid solution is effectively removed and the loss of phosphate is avoided, thereby achieving a higher phosphate recovery rate.

[0049] (2) In the method provided by the present invention, on the one hand, sulfate is separated in the form of calcium sulfate dihydrate, and the obtained calcium sulfate dihydrate can be used as a valuable product. On the other hand, phosphate is recovered and converted into potassium dihydrogen phosphate, which not only reduces waste discharge, but also maximizes resource utilization, significantly improves economic benefits, avoids the impact of toxic desulfurization agents on the environment, and has great potential in environmental protection and resource recycling.

[0050] (3) In the method provided by the present invention, the purity of potassium dihydrogen phosphate can reach more than 60.8%, and the recovery rate of phosphate can reach more than 76.3%. Under optimal conditions, the purity of potassium dihydrogen phosphate can reach more than 98.28%, meeting the requirements of first-class products, and the recovery rate of phosphate can reach more than 98.2%; at the same time, sulfate can also be produced in the form of calcium sulfate dihydrate, and the purity of the obtained calcium sulfate dihydrate reaches more than 58%, and can reach more than 98% under optimal conditions. DETAILED DESCRIPTION

[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0052] Example 1

[0053] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid, the method comprising the following steps:

[0054] (1) 5 L of a phosphorus-sulfur mixed acid solution having a pH value of 1, a phosphate concentration of 1800 g / L, and a sulfate concentration of 300 g / L was taken, and the phosphorus-sulfur mixed acid solution and slaked lime were mixed at a temperature of 30° C. The mixing was performed by dividing the lime into 10 batches, and adding the slaked lime to the phosphorus-sulfur mixed acid solution in such a manner that the mass of slaked lime added in each batch accounted for 10% of the total mass of slaked lime, and the time interval between each batch was 15 min. During the mixing, the Ca(OH)2 in the slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution were controlled to be 100 g / L. 2-The molar ratio of the amount of the slaked lime is 1:1.25 (i.e., a total of 1445 g of slaked lime is added), the mixing process is stirred for 4 hours, and then filtered to obtain a filtrate and a filter residue containing calcium sulfate dihydrate, and the filter residue containing calcium sulfate dihydrate is washed with 500 mL of 55° C. water to obtain a washed liquid and calcium sulfate dihydrate;

[0055] (2) mixing the washed liquid and the filtrate obtained in step (1), and then adding potassium hydroxide to adjust the pH value to an end point pH value of 6.5 to obtain a potassium-containing solution;

[0056] (3) distilling the potassium-containing solution obtained in step (2) until the solution has a specific gravity of 1.6, adding phosphoric acid to the mother liquor obtained by distillation to adjust the pH value to an end point pH value of 4.4, then cooling to an end point temperature of 38° C., and then centrifuging to obtain a potassium dihydrogen phosphate product.

[0057] Ion chromatography was used to detect the P content, S content, phosphate content, and sulfate content in the phosphorus-sulfur mixed acid solution, filtrate, washed liquid, and a solution obtained by mixing the washed liquid and filtrate in this embodiment. The results are shown in Table 1.

[0058] Table 1

[0059]

[0060] According to the data in Table 1, the recovery rate of phosphate in this embodiment (the recovery rate of phosphate in the present invention refers to the ratio of the mass of phosphate in the mixed solution of the cleaning liquid and the filtrate to the mass of phosphate in the phosphorus-sulfur mixed acid solution) reached 98.3%, and the mass ratio of phosphate to sulfate in the solution obtained by mixing the cleaning liquid and the filtrate was 31.15:1.

[0061] Example 2

[0062] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid, the method comprising the following steps:

[0063] (1) 5 L of a phosphorus-sulfur mixed acid solution having a pH value of 1, a phosphate concentration of 1800 g / L, and a sulfate concentration of 300 g / L was taken, and the phosphorus-sulfur mixed acid solution and slaked lime were mixed at a temperature of 20° C. The mixing was performed by dividing the lime into 5 batches, and adding the slaked lime to the phosphorus-sulfur mixed acid solution in such a manner that the mass of slaked lime added in each batch accounted for 20% of the total mass of slaked lime, and the time interval between each batch was 10 min. During the mixing, the Ca(OH)2 in the slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution were controlled to be 1:1. 2-The molar ratio of the amount of the slaked lime is 1:1.3 (i.e., a total of 1503 g of slaked lime is added), the mixing process is stirred for 5 hours, and then filtered to obtain a filtrate and a filter residue containing calcium sulfate dihydrate, and the filter residue containing calcium sulfate dihydrate is washed with 500 mL of 50° C. water to obtain a washed liquid and calcium sulfate dihydrate;

[0064] (2) mixing the washed liquid and the filtrate obtained in step (1), and then adding potassium hydroxide to adjust the pH value to an end point pH value of 6 to obtain a potassium-containing solution;

[0065] (3) distilling the potassium-containing solution obtained in step (2) until the solution has a specific gravity of 1.7, adding phosphoric acid to the mother liquor obtained by distillation to adjust the pH value to an end point pH value of 4.2, then cooling to an end point temperature of 40° C., and then centrifuging to obtain a potassium dihydrogen phosphate product.

[0066] Ion chromatography was used to detect the P content, S content, phosphate content, and sulfate content in the phosphorus-sulfur mixed acid solution, filtrate, washed liquid, and a solution obtained by mixing the washed liquid and filtrate in this example. The results are shown in Table 2.

[0067] Table 2

[0068]

[0069] According to the data in Table 2, the recovery rate of phosphate in this embodiment reaches 98.2%, and the mass ratio of phosphate to sulfate in the solution obtained by mixing the washed liquid and the filtrate is 33.35:1.

[0070] Example 3

[0071] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid, the method comprising the following steps:

[0072] (1) 5 L of a phosphorus-sulfur mixed acid solution having a pH value of 1, a phosphate concentration of 1800 g / L, and a sulfate concentration of 300 g / L was taken, and the phosphorus-sulfur mixed acid solution and slaked lime were mixed at a temperature of 45° C. The mixing was performed by dividing the lime into 10 batches, and adding the slaked lime to the phosphorus-sulfur mixed acid solution in such a manner that the mass of slaked lime added in each batch accounted for 10% of the total mass of slaked lime, and the time interval between each batch was 5 min. During the mixing, the Ca(OH)2 in the slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution were controlled to be 100 μg / L. 2- The molar ratio of the amount of the slaked lime is 1:1.5 (i.e., a total of 1734 g of slaked lime is added), the mixing process is stirred for 6 hours, and then filtered to obtain a filtrate and a filter residue containing calcium sulfate dihydrate, and the filter residue containing calcium sulfate dihydrate is washed with 500 mL of 60° C. water to obtain a washed liquid and calcium sulfate dihydrate;

[0073] (2) mixing the washed liquid and the filtrate obtained in step (1), wherein the mass ratio of phosphate to sulfate in the solution is 35:1, and then adding potassium hydroxide to adjust the pH value to an end point pH value of 7 to obtain a potassium-containing solution;

[0074] (3) distilling the potassium-containing solution obtained in step (2) until the solution has a specific gravity of 1.5, adding phosphoric acid to the mother liquor obtained by distillation to adjust the pH value to an end point pH value of 4.5, then cooling to an end point temperature of 35° C., and then centrifuging to obtain a potassium dihydrogen phosphate product.

[0075] Ion chromatography was used to detect the P content, S content, phosphate content, and sulfate content in the phosphorus-sulfur mixed acid solution, filtrate, washed liquid, and a solution obtained by mixing the washed liquid and filtrate in this example. The results are shown in Table 3.

[0076] Table 3

[0077]

[0078]

[0079] According to the data in Table 3, the recovery rate of phosphate in this embodiment reaches 99.33%, and the mass ratio of phosphate to sulfate in the solution obtained by mixing the washed liquid and the filtrate is 35:1.

[0080] Example 4

[0081] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid. The difference between the method and embodiment 1 is that the amount of slaked lime added is adjusted so that the Ca(OH)2 in the slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution are 2- The molar ratio of phosphate to sulfate is 1:1, and the mass ratio of phosphate to sulfate in the solution obtained by mixing the washed liquid and the filtrate is 21.04:1.

[0082] Example 5

[0083] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid. The difference between the method and embodiment 1 is that the amount of slaked lime added is adjusted so that the Ca(OH)2 in the slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution are 2- The molar ratio of phosphate to sulfate is 1:1.6, and the mass ratio of phosphate to sulfate in the solution obtained by mixing the washing liquid and the filtrate is 37.2:1.

[0084] Example 6

[0085] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid. The difference between the method and embodiment 1 is that the pH value of the phosphorus-sulfur mixed acid solution is 2.

[0086] Example 7

[0087] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid. The difference between the method and embodiment 1 is that the mixing temperature in step (1) is controlled to be 15°C.

[0088] Example 8

[0089] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid. The difference between the method and embodiment 1 is that the mixing temperature in step (1) is controlled to be 60°C.

[0090] Example 9

[0091] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid. The difference between the method and embodiment 1 is that the stirring time in step (1) is 3 hours.

[0092] Example 10

[0093] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfur mixed acid. The difference between the method and Example 1 is that the time interval for adding each batch in step (1) is 2 minutes.

[0094] Embodiment 11

[0095] This embodiment provides a method for resource recovery of phosphoric acid in phosphorus-sulfuric acid mixed acid. The difference between the method and embodiment 1 is that in step (1), all the slaked lime is directly added to the phosphorus-sulfuric acid mixed acid solution at one time.

[0096] The recovery rate of phosphate in Examples 1-11 was calculated, and the results are shown in Table 1; the composition and content of the potassium dihydrogen phosphate product in Examples 1-11 and the purity of calcium sulfate dihydrate were determined by acid-base titration and disodium EDTA (ethylenediaminetetraacetic acid) titration, and the results are shown in Table 1.

[0097] Table 1

[0098]

[0099]

[0100] From the data in Table 1, we can see the following points:

[0101] (1) It can be seen from the data of Examples 1-11 that the method provided by the present invention can recover phosphate and convert it into potassium dihydrogen phosphate. The purity of potassium dihydrogen phosphate reaches more than 60.8%, and the recovery rate of phosphate reaches more than 76.3%. Under optimal conditions, the purity of potassium dihydrogen phosphate reaches more than 98.28%, meeting the requirements of first-class products, and the recovery rate of phosphate reaches more than 98.2%; at the same time, sulfate can also be produced in the form of calcium sulfate dihydrate. The purity of the obtained calcium sulfate dihydrate reaches more than 58%, and can reach more than 98% under optimal conditions.

[0102] (2) Comprehensive comparison of the data of Example 1 and Examples 4-5 shows that the difference between Example 4-5 and Example 1 is only that the Ca(OH)2 in the slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution 2- The molar ratio of phosphate to sulfate in the solution obtained by mixing the washing liquid and the filtrate is not within the preferred range of the present invention, which further leads to the mass ratio of phosphate to sulfate in the solution obtained by mixing the washing liquid and the filtrate being not within the preferred range of the present invention. The recovery rate of phosphate and the purity of potassium dihydrogen phosphate in Example 1 are significantly higher than those in Examples 4-5, and the purity of calcium sulfate dihydrate in Example 1 is higher than that in Example 4. It can be seen that the present invention achieves the desired effect by preferably controlling the Ca(OH)2 in slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution. 2- The molar ratio of can further promote the separation of phosphate and sulfate, obtain higher purity potassium dihydrogen phosphate product and calcium sulfate dihydrate product, and improve the recovery rate of phosphate.

[0103] (3) A comprehensive comparison of the data of Example 1 and Example 6 shows that the only difference between Example 6 and Example 1 is that the pH value of the phosphorus-sulfur mixed acid is not within the preferred range of the present invention. The recovery rate of phosphate and the purity of potassium dihydrogen phosphate in Example 1 are significantly higher than those in Example 6, and the purity of calcium sulfate dihydrate is also significantly higher than that in Example 6. It can be seen that the present invention can further improve the recovery rate of phosphate, the purity of potassium dihydrogen phosphate, and the purity of calcium sulfate dihydrate by preferably controlling the pH value of the phosphorus-sulfur mixed acid.

[0104] (4) A comprehensive comparison of the data of Example 1 and Examples 7-8 shows that the only difference between Example 7-8 and Example 1 is that the temperature of controlling the mixing in step (1) is not within the preferred range of the present invention. The recovery rate of phosphate and the purity of potassium dihydrogen phosphate in Example 1 are significantly higher than those in Example 7-8, and the purity of calcium sulfate dihydrate is also significantly higher than that in Example 7-8. It can be seen that the present invention can further improve the recovery rate of phosphate, the purity of potassium dihydrogen phosphate, and the purity of calcium sulfate dihydrate by preferably controlling the mixing temperature in step (1).

[0105] (5) Comprehensive comparison of the data of Example 1 and Examples 9-11 shows that the recovery rate of phosphate and the purity of potassium dihydrogen phosphate in Example 1 are significantly higher than those in Examples 9-11, and the purity of calcium sulfate dihydrate is also significantly higher than that in Examples 9-11. It can be seen that the present invention can control the mixing process to adapt to the viscosity and temperature changes of the reactants by preferably controlling the addition of slaked lime to the mixed acid solution in batches, and further controlling the stirring time, the time interval between the addition of each batch, etc., so as to promote the full reaction of sulfate and avoid the loss of phosphate, and further ensure the purity of subsequent potassium dihydrogen phosphate and the recovery rate of phosphate, as well as the purity of calcium sulfate dihydrate.

[0106] In summary, the method provided by the present invention can effectively separate sulfate from the mixed acid solution and significantly reduce the loss of phosphate, thereby realizing the resource utilization of phosphoric acid in phosphorus-sulfur mixed acid, avoiding the impact of toxic desulfurizers on the environment, and significantly improving economic benefits.

[0107] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for recycling phosphoric acid in phosphorus-sulfur mixed acid, characterized in that: The method comprises the following steps: (1) mixing a phosphorus-sulfur mixed acid solution and slaked lime, and then performing solid-liquid separation to obtain a filtrate and a filter residue containing calcium sulfate dihydrate; (2) mixing the filtrate obtained in step (1) with potassium hydroxide to adjust the pH value to obtain a potassium-containing solution; (3) distilling the potassium-containing solution obtained in step (2), adding phosphoric acid to the distillation mother liquor obtained by the distillation to adjust the pH value, and then cooling and solid-liquid separation are performed in sequence to obtain a potassium dihydrogen phosphate product.

2. The method according to claim 1, characterized in that The mass ratio of phosphate to sulfate in the phosphorus-sulfur mixed acid solution in step (1) is greater than 3.

3. The method according to claim 1 or 2, characterized in that: The mixing in step (1) is carried out under the condition of pH value <1.5; Preferably, the mixing temperature in step (1) is controlled to be 20-50°C; Preferably, stirring is performed during the mixing process in step (1); Preferably, the stirring time is 4-6 hours.

4. The method according to any one of claims 1 to 3, characterized in that: The mixing of step (1) controls the Ca(OH)2 in the slaked lime and the SO4 in the phosphorus-sulfur mixed acid solution. 2- The molar ratio is 1:(1.25-1.5).

5. The method according to any one of claims 1 to 4, characterized in that: The mixing in step (1) comprises adding slaked lime to the phosphorus-sulfur mixed acid solution in batches; Preferably, the mass of slaked lime added in each batch accounts for 5-10% of the total mass of slaked lime; Preferably, the time interval between adding each batch is 5-15 minutes.

6. The method according to any one of claims 1 to 5, characterized in that: The calcium sulfate dihydrate-containing filter residue in step (1) is washed to obtain a washed liquid and calcium sulfate dihydrate; Preferably, the filtrate is mixed with the washed solution, and potassium hydroxide is then added to adjust the pH value; Preferably, the mass ratio of phosphate to sulfate in the solution obtained by mixing the filtrate and the washed liquid is (28-35):

1.

7. The method according to claim 6, characterized in that The washing liquid used in the washing in step (1) comprises water; Preferably, the water temperature used for the cleaning is 50-60°C.

8. The method according to any one of claims 1 to 7, characterized in that: The end point pH value of the pH adjustment in step (2) is 6-7.

9. The method according to any one of claims 1 to 8, characterized in that: Step (3) wherein the solution is distilled to a specific gravity of 1.5-1.7; Preferably, the endpoint pH value of the pH adjustment is 4.2-4.5; Preferably, the cooling to the terminal temperature is 35-40°C.

10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) mixing a phosphorus-sulfuric acid solution and slaked lime at a pH value of less than 1.5 and a temperature of 20-50° C., wherein the mixing comprises adding slaked lime to the phosphorus-sulfuric acid solution in a manner such that the mass of slaked lime added in each batch accounts for 5-10% of the total mass of slaked lime and the time interval between each batch is 5-15 minutes, and the mixing is controlled to reduce the Ca(OH)2 in the slaked lime to SO4 in the phosphorus-sulfuric acid solution. 2- The molar ratio of the mixture is 1:(1.25-1.5), the mixing process is stirred for 4-6 hours, and then the solid-liquid separation is performed to obtain a filtrate and a filter residue containing calcium sulfate dihydrate, the filter residue containing calcium sulfate dihydrate is washed to obtain a washed liquid and calcium sulfate dihydrate, and the water temperature used for the washing is 50-60°C; (2) mixing the cleaned liquid and the filtrate obtained in step (1), wherein the mass ratio of phosphate to sulfate in the obtained solution is (28-35):1, and then adding potassium hydroxide to adjust the pH value to an end point pH value of 6-7 to obtain a potassium-containing solution; (3) distilling the potassium-containing solution obtained in step (2) until the solution has a specific gravity of 1.5-1.7, adding phosphoric acid to the mother liquor obtained by distillation to adjust the pH value to an end point pH value of 4.2-4.5, then cooling to an end point temperature of 35-40° C., and then solid-liquid separation to obtain a potassium dihydrogen phosphate product.

Citation Information

Patent Citations

  • Resource utilization method of waste sulfuric acid liquid containing phosphoric acid

    CN114195178A

  • Method for producing potassium dihydrogen phosphate through wet-process phosphoric acid

    CN103072963A

  • Method for recovering high purity calcium hydrogen phosphate in sulfur acid-containing waste phosphoric acid

    CN103738933A

  • Method for producing potassium dihydrogen phosphate and potassium-ammonium dihydrogen phosphate through wet process phosphoric acid

    CN105000539A

  • Process for producing monopotassium phosphate and calcium sulfate whiskers from phosphorite

    CN115092900A