Iron phosphate with high iron-phosphorus ratio and preparation method thereof

By introducing ammonium metavanadate into the conversion reaction of iron phosphate, the pH of the system is adjusted to form polyvanadate, and the iron content and iron-phosphorus ratio of iron phosphate are improved, the problem of limited increase in iron-phosphorus ratio in the existing technology is solved, and the problem of significantly improving the iron-phosphorus ratio is significantly improved. The electrochemical properties of lithium iron phosphate positive electrode material.

CN118929602APending Publication Date: 2024-11-12ZHEJIANG YOUSHAN NEW MATERIAL TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411214963.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to improve the iron-phosphorus ratio of iron phosphate materials in large-scale production, resulting in limited electrochemical performance, and the iron-phosphorus of most iron phosphate products on the market is lower than 0.980.

Method used

By introducing ammonium metavanadate as an additive, the pH of the system is adjusted during the conversion reaction, forming a reaction between polyvanadate and trivalent iron ions, increasing the iron content and iron-phosphorus ratio of iron phosphate, and adjusting the amount of ammonium metavanadate added Accurate regulation within the range of 0.980-0.990.

Benefits of technology

Effectively improve the iron content and iron-phosphorus ratio of iron phosphate, and improve its electrochemical performance. In particular, the 1C discharge specific capacity of lithium iron phosphate positive electrode material can reach 150 mAh/g, and is suitable for different iron phosphate preparation process routes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929602A_ABST
    Figure CN118929602A_ABST
Patent Text Reader

Abstract

The invention provides iron phosphate with a high iron-phosphorus ratio and a preparation method thereof.The preparation method comprises the following steps that S1, a synthesis reaction is conducted, specifically, a hydrogen peroxide solution, a ferrite solution and a phosphorus salt solution are prepared, pure water serves as a reaction kettle base solution, and yellow slurry A is obtained through the synthesis reaction; s2, conversion reaction: respectively preparing a phosphoric acid solution and an ammonium metavanadate solution, and carrying out solid-liquid separation and washing treatment on the yellow slurry A to obtain a yellow filter cake A; mixing the yellow filter cake A with pure water for slurrying, then adding a phosphoric acid solution and an ammonium metavanadate solution, carrying out heating and heat preservation treatment, carrying out conversion reaction to obtain white slurry B, and carrying out solid-liquid separation and washing treatment on the white slurry B to obtain a white filter cake B; s3, drying and calcining: carrying out flash evaporation drying, calcining and crushing treatment on the white filter cake B to obtain an iron phosphate material with a high iron-phosphorus ratio; according to the iron phosphate prepared by the method provided by the invention, the iron content and the iron-phosphorus ratio of the iron phosphate are effectively improved, and the electrochemical performance of the corresponding lithium iron phosphate positive electrode material is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of batteries, and in particular to high iron-phosphorus ratio ferric phosphate and a preparation method thereof. Background Art

[0002] In the solid-phase process of preparing lithium iron phosphate with raw materials such as iron phosphate, lithium carbonate, and glucose, the physical and chemical indicators of iron phosphate, especially key indicators such as the iron-phosphorus ratio, have an important influence on the electrochemical properties of lithium iron phosphate. Generally speaking, the higher the iron-phosphorus ratio of the precursor iron phosphate, the better the electrochemical performance of the corresponding lithium iron phosphate positive electrode material. The current high iron-phosphorus ratio iron phosphate preparation technology usually regulates the reaction parameters in a direction that is conducive to the growth and improvement of iron phosphate crystals to increase the iron-phosphorus ratio of the iron phosphate material. However, due to the constraints of actual production conditions, there are limits to the range in which each reaction parameter can be controlled, and there is limited room for improvement in the iron-phosphorus ratio. At present, the iron-phosphorus ratio of most iron phosphate products produced on the market on a large scale is lower than 0.980. Summary of the invention

[0003] The present invention provides a method for preparing ferric phosphate with a high iron-phosphorus ratio to solve the above technical problems, which is specifically as follows: S1, synthesis reaction: prepare hydrogen peroxide solution, ferrous salt solution, and phosphate solution respectively, use pure water as the bottom liquid of the reactor, add the hydrogen peroxide solution, phosphate solution, and ferrous salt solution into the reactor, and obtain yellow slurry A through synthesis reaction; S2, conversion reaction: prepare phosphoric acid solution and ammonium metavanadate solution respectively, perform solid-liquid separation and washing treatment on the yellow slurry A obtained in step S1 to obtain yellow filter cake A; mix the yellow filter cake A with pure water to make a slurry, then add phosphoric acid solution to adjust the pH of the slurry, then add ammonium metavanadate solution, then heat and keep the temperature, obtain white slurry B through conversion reaction, and obtain white filter cake B after solid-liquid separation and washing treatment of white slurry B; S3, drying and calcining: flash drying, calcining and crushing the white filter cake B obtained in step S2 to obtain an iron phosphate material with a high iron-phosphorus ratio; The methods and equipment for solid-liquid separation and washing treatment of yellow slurry A in S2 are common methods and equipment in the industry; the methods and equipment for solid-liquid separation and washing treatment of white slurry B are common methods and equipment in the industry; the methods and equipment for flash drying, calcination and crushing of filter cake C in S3 are also common methods and equipment in the industry.

[0004] Moreover, in step S1, the mass concentration of the hydrogen peroxide solution is 10-30wt%, the concentration of the ferrous salt solution is 0.5-2.0 mol / L, and the concentration of the phosphate solution is 0.5-2.0 mol / L.

[0005] Moreover, in step S1, the pH of the synthesis reaction is ≤2.5, the purpose of which is to avoid the formation of precipitates such as ferric hydroxide, ferrous hydroxide, and ferrous phosphate during the synthesis process.

[0006] Moreover, in the step S1, the ferrous salt solution is prepared from any one of ferrous sulfate, ferrous nitrate, ferrous chloride, iron powder, and iron sheet as a raw material; the phosphate salt solution is prepared from any one of ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, and phosphoric acid as a raw material.

[0007] Moreover, in the step S1, the molar ratio of the hydrogen peroxide in the hydrogen peroxide solution to the molar ratio of the iron element in the ferrous salt solution is n(Fe):n(H 2 O 2 )=1:0.5-1:1.

[0008] Moreover, in the step S1, the molar ratio of the phosphorus element in the phosphate salt solution to the iron element in the ferrous salt solution is n(Fe):n(P)=1:0.9-1:1.2.

[0009] Moreover, in the step S2, after the phosphoric acid solution is added, the pH of the slurry is controlled to be 1.6-2.0, and the pH of the slurry is controlled by adjusting the amount of phosphoric acid.

[0010] Moreover, in step S2, the amount of ammonium metavanadate added is controlled to be n(V):n(Fe)=0.3%-1.5%.

[0011] Moreover, in step S2, the specific method of heating and heat preservation treatment is: heating to 90-100° C. and then keeping the temperature for 2-4 hours.

[0012] On the other hand, the present invention provides iron phosphate prepared by a method for preparing high iron-phosphorus ratio iron phosphate, wherein the iron-phosphorus ratio of the iron phosphate is greater than 0.980; and the vanadium content in the iron phosphate is 1500-5000 ppm.

[0013] The present invention aims to provide a high iron-phosphorus ratio ferric phosphate and a preparation method thereof. The principle of the scheme provided by the present invention to obtain a high iron-phosphorus ratio is that: the present invention introduces ammonium metavanadate as an additive in the conversion stage. During the conversion reaction, since the pH of the system is at a relatively low level (pH≤2.5), the metavanadate will be converted into the formation of polyvanadate. During the ferric phosphate conversion reaction, the polyvanadate will react with trivalent iron ions to form ferric vanadate, thereby effectively improving Fe% and Fe / P (10Fe 3+ + H 2 V 10 O 28 4- + 26OH - → 10FeVO 4 ·4H2 O +10H 2 O).

[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. The method for preparing ferric phosphate with a high iron-to-phosphorus ratio provided by the present invention can be applied to different ferric phosphate preparation process routes in the industry, such as: ammonium method, sodium method, iron method, etc. The key to the method for preparing ferric phosphate with a high iron-to-phosphorus ratio provided by the present invention is to introduce ammonium metavanadate as an additive, and the process route or main process parameters are not limited.

[0015] 2. The present invention provides a method for preparing ferric phosphate with a high iron-to-phosphorus ratio, which effectively improves the iron content and iron-to-phosphorus ratio of the ferric phosphate. By adjusting the amount of ammonium metavanadate added, the iron-to-phosphorus ratio can be accurately controlled within the range of 0.980-0.9900.

[0016] 3. The present invention provides a method for preparing high iron-phosphorus ratio iron phosphate, which can increase the iron-phosphorus ratio to above 0.980, which is beneficial to improving the electrochemical performance of the corresponding lithium iron phosphate positive electrode material. On the other hand, due to the introduction of V element, the iron phosphate material prepared by the present invention is used to prepare lithium iron phosphate, and a small amount of Li 3 V 2 (PO 4 ) 3 , further improving the electrochemical performance of the positive electrode material, and the 1C discharge specific capacity can reach 150 mAh / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a graph showing the trend of the iron content of the finished ferrous phosphate product changing with the amount of vanadium added; Figure 2 XRD of lithium iron phosphate prepared from iron phosphate of Examples 1 to 5 and Comparative Example 3; Figure 3 This is a partial enlarged XRD diagram of lithium iron phosphate prepared from the iron phosphate of Examples 1 to 5 and Comparative Example 3. DETAILED DESCRIPTION

[0018] Example 1 A method for preparing ferric phosphate with a high iron-phosphorus ratio, the preparation process comprising the following steps: S1. Synthesis reaction: Prepare 180 L of ferrous solution with a molar concentration of 0.8 mol / L of iron and 150 L of phosphate solution with a molar concentration of 1 mol / L of phosphorus. Add the ferrous solution, phosphate solution and hydrogen peroxide solution into the reactor under stirring to control the ratio of n(Fe):n(H 2 O 2 )=1:0.55, and a yellow slurry A was obtained through synthesis reaction; S2, conversion reaction: the yellow slurry A is subjected to solid-liquid separation and washing treatment to obtain a yellow filter cake A; the filter cake A is mixed with pure water and slurried, and then a phosphoric acid solution is added to adjust the slurry pH to 1.8, and an ammonium metavanadate solution is added to control n(V):n(Fe)=0.4%, and then the temperature is raised to 92°C and kept warm for 3.0 h, and a white slurry B is obtained through a conversion reaction; S3, drying and calcining: subjecting the white slurry B to solid-liquid separation and washing treatment to obtain a filter cake white filter cake B; subjecting the filter cake B to flash drying, calcination, and crushing treatment to obtain iron phosphate with a high iron-phosphorus ratio.

[0019] Example 2 A method for preparing ferric phosphate with a high iron-phosphorus ratio, the preparation process comprising the following steps: S1. Synthesis reaction: Prepare 180 L of ferrous solution with a molar concentration of 0.8 mol / L of iron and 150 L of phosphate solution with a molar concentration of 1 mol / L of phosphorus. Add the ferrous solution, phosphate solution and hydrogen peroxide solution into the reactor under stirring to control the ratio of n(Fe):n(H 2 O 2 )=1:1, and a yellow slurry A is obtained through a synthetic reaction; S2, conversion reaction: the yellow slurry A is subjected to solid-liquid separation and washing treatment to obtain a yellow filter cake A; the filter cake A is mixed with pure water and slurried, and then a phosphoric acid solution is added to adjust the slurry pH to 1.8, and n(V):n(Fe)=0.5% is controlled, and an ammonium metavanadate solution is added, and the temperature is raised to 95°C and kept warm for 2.5 hours, and a white slurry B is obtained through a conversion reaction; S3, drying and calcining: subjecting the white slurry B to solid-liquid separation and washing treatment to obtain a filter cake white filter cake B; subjecting the filter cake B to flash drying, calcination, and crushing treatment to obtain iron phosphate with a high iron-phosphorus ratio.

[0020] Example 3 A method for preparing ferric phosphate with a high iron-phosphorus ratio, the preparation process comprising the following steps: S1. Synthesis reaction: Prepare 180 L of ferrous solution with a molar concentration of 0.8 mol / L of iron and 150 L of phosphate solution with a molar concentration of 1 mol / L of phosphorus. Add the ferrous solution, phosphate solution and hydrogen peroxide solution into the reactor under stirring to control the ratio of n(Fe):n(H 2 O 2 )=1:0.65, and a yellow slurry A was obtained through synthesis reaction; S2, conversion reaction: the yellow slurry A is subjected to solid-liquid separation and washing treatment to obtain a yellow filter cake A; the filter cake A is mixed with pure water and slurried, and then a phosphoric acid solution is added to adjust the slurry pH to 1.8, and n(V):n(Fe)=0.55% is controlled, and an ammonium metavanadate solution is added, and the temperature is raised to 90°C and kept for 2 hours, and a white slurry B is obtained through a conversion reaction; S3, drying and calcining: subjecting the white slurry B to solid-liquid separation and washing treatment to obtain a filter cake white filter cake B; subjecting the filter cake B to flash drying, calcination, and crushing treatment to obtain iron phosphate with a high iron-phosphorus ratio.

[0021] Example 4 A method for preparing ferric phosphate with a high iron-phosphorus ratio, the preparation process comprising the following steps: S1. Synthesis reaction: Prepare 180 L of ferrous solution with a molar concentration of 0.8 mol / L of iron and 150 L of phosphate solution with a molar concentration of 1 mol / L of phosphorus. Add the ferrous solution, phosphate solution and hydrogen peroxide solution into the reactor under stirring to control the ratio of n(Fe):n(H 2 O 2 )=1:0.65, and a yellow slurry A was obtained through synthesis reaction; S2, conversion reaction: the yellow slurry A is subjected to solid-liquid separation and washing treatment to obtain a yellow filter cake A; the filter cake A is mixed with pure water and slurried, and then a phosphoric acid solution is added to adjust the slurry pH to 1.8, and n(V):n(Fe)=1.10% is controlled, and an ammonium metavanadate solution is added, and the temperature is raised to 94°C and kept warm for 2.5 hours, and a white slurry B is obtained through a conversion reaction; S3, drying and calcining: subjecting the white slurry B to solid-liquid separation and washing treatment to obtain a filter cake white filter cake B; subjecting the filter cake B to flash drying, calcination, and crushing treatment to obtain iron phosphate with a high iron-phosphorus ratio.

[0022] Example 5 A method for preparing ferric phosphate with a high iron-phosphorus ratio, the preparation process comprising the following steps: S1. Synthesis reaction: Prepare 180 L of ferrous solution with a molar concentration of 0.8 mol / L of iron and 150 L of phosphate solution with a molar concentration of 1 mol / L of phosphorus. Add the ferrous solution, phosphate solution and hydrogen peroxide solution into the reactor under stirring to control the ratio of n(Fe):n(H 2 O 2 )=1:0.65, and a yellow slurry A was obtained through synthesis reaction; S2, conversion reaction: the yellow slurry A is subjected to solid-liquid separation and washing treatment to obtain a yellow filter cake A; the filter cake A is mixed with pure water and slurried, and then a phosphoric acid solution is added to adjust the slurry pH to 1.8, and n(V):n(Fe)=1.40% is controlled, and an ammonium metavanadate solution is added, and the temperature is raised to 93°C and kept warm for 3.0 h, and a white slurry B is obtained through a conversion reaction; S3, drying and calcining: subjecting the white slurry B to solid-liquid separation and washing treatment to obtain a filter cake white filter cake B; subjecting the filter cake B to flash drying, calcination, and crushing treatment to obtain iron phosphate with a high iron-phosphorus ratio.

[0023] Comparative Example 1 The process parameters of this comparative example are consistent with those of Example 1, except that no ammonium metavanadate solution is added in step S2.

[0024] Comparative Example 2 The process parameters of this comparative example are consistent with those of Example 1, except that the amount of ammonium metavanadate solution added in step S2 of this comparative example is controlled to be n(V):n(Fe)=0.28%.

[0025] Comparative Example 3 The process parameters of this comparative example are consistent with those of Example 1, except that the amount of ammonium metavanadate solution added in step S2 of this comparative example is controlled to be n(V):n(Fe)=1.6%.

[0026] Experimental Section

[0027] Experiment 1 The iron-phosphorus ratios of the iron phosphates obtained in Examples 1 to 5 and Comparative Examples 1 to 3 were tested, as shown in Table 1.

[0028] Table 1 Iron content and iron-phosphorus ratio of ferric phosphate

[0029] It can be seen from Table 1 that when ammonium metavanadate is not added, the iron content and iron-phosphorus ratio of iron phosphate are low. As the amount of ammonium metavanadate added increases, the vanadium content in the prepared iron phosphate gradually increases, and the iron content and iron-phosphorus ratio of the prepared iron phosphate gradually increase. When the amount of ammonium metavanadate added makes n(V):n(Fe)=1.60%, the iron content and iron-phosphorus of the iron phosphate decrease.

[0030] Figure 1The figure shows the changing trend of the iron content in the finished iron phosphate product with the vanadium content. It can be seen from the figure that there is a significant linear correlation between the iron content and the vanadium content of the finished product. Adjusting the amount of ammonium metavanadate can achieve the purpose of adjusting the iron content and the iron-phosphorus ratio of the finished product. During the experiment, it was found that when the vanadium content in the finished iron phosphate product is less than 1500ppm, the iron-phosphorus ratio in the iron phosphate will be lower than 0.980; and when the vanadium content in the finished iron phosphate product is greater than 5000ppm, the crystal structure will be affected, and the iron-phosphorus ratio in the iron phosphate will eventually be lower than 0.980. Therefore, when the vanadium content in the finished iron phosphate product is 1500ppm-5000ppm, the effect of the finished iron phosphate product is best.

[0031] The iron phosphate prepared in each embodiment and comparative example is used as a precursor to prepare lithium iron phosphate. Figure 2 The XRD patterns of lithium iron phosphate prepared from iron phosphate of Examples 1 to 5 and Comparative Example 3 are shown. Figure 3 The partial enlarged view (35°-36°) of the XRD spectrum of lithium iron phosphate made from iron phosphate in Examples 1 to 5 and Comparative Example 3 is shown. It can be seen from the figure that when the vanadium doping amount in iron phosphate is 1500-5000 ppm, it does not affect the crystal structure of lithium iron phosphate. When the vanadium doping amount in iron phosphate exceeds 5000 ppm, the characteristic peak at the position of 36.01° will shift significantly to the left, indicating that excessive vanadium doping will lead to a narrowing of the interlayer spacing and lattice contraction of lithium iron phosphate. In theory, too narrow interlayer spacing is not conducive to the deintercalation and diffusion of lithium ions, and will have an adverse effect on the electrochemical properties of lithium iron phosphate.

[0032] Experiment 2 Lithium iron phosphate prepared from the iron phosphate prepared in Examples 1 to 5 and Comparative Examples 1 to 3 of the present invention was made into button batteries, and the first discharge specific capacity of the batteries under 0.1C and 1C conditions was tested. The specific results are shown in Table 2.

[0033] Table 2 Lithium iron phosphate performance test results

[0034] It can be seen from Table 2 that the 1C discharge capacities of Example 1, Example 2, Example 3, Example 4, and Example 5 are 149.13, 149.08, 149.22, 151.35, and 152.41 mAh / g, respectively, and the discharge capacities of Comparative Example 1, Comparative Example 2, and Comparative Example 3 are 145.01, 147.24, and 143.04 mAh / g, respectively.

[0035] When the vanadium doping amount is 1500-5000 ppm, as the vanadium doping amount in iron phosphate increases, the 1C discharge capacity of lithium iron phosphate gradually increases. On the one hand, this may be because with the increase of vanadium doping, the iron content of iron phosphate increases, which is beneficial to the improvement of the electrochemical performance of lithium iron phosphate; on the other hand, it may be because appropriate vanadium doping is conducive to the formation of a small amount of lithium vanadium phosphate material with fast charging and discharging characteristics, which improves the lithium ion diffusion rate and conductivity, and promotes the improvement of 1C discharge capacity.

[0036] It is worth noting that when the vanadium content exceeds 5000 ppm (Comparative Example 3), the 1C discharge capacity is significantly reduced to only 143.04 mAh / g. The lithium iron phosphate prepared by the iron phosphate in Examples 1 to 5 and Comparative Example 3 is subjected to X-ray analysis, and the obtained XRD pattern is as follows: Figure 2 , Figure 3 As shown, combined Figure 2 and Figure 3 The results show that when the vanadium doping amount is too high, the characteristic peak in the lithium iron phosphate XRD spectrum will shift to the left and the interlayer spacing will narrow, which limits the extraction and embedding of lithium ions and thus has an adverse effect on the electrochemical performance.

Claims

1. A method for preparing ferric phosphate with a high iron-to-phosphorus ratio, characterized in that: The following steps are involved: S1, synthesis reaction: prepare hydrogen peroxide solution, ferrous salt solution, and phosphate solution respectively, use pure water as the bottom liquid of the reactor, add the hydrogen peroxide solution, phosphate solution, and ferrous salt solution into the reactor, and obtain yellow slurry A through synthesis reaction; S2, conversion reaction: prepare phosphoric acid solution and ammonium metavanadate solution respectively, perform solid-liquid separation and washing treatment on the yellow slurry A obtained in step S1 to obtain yellow filter cake A; mix the yellow filter cake A with pure water for pulping, then add phosphoric acid solution and ammonium metavanadate solution, perform heating and heat preservation treatment, obtain white slurry B through conversion reaction, and obtain white filter cake B after solid-liquid separation and washing treatment of white slurry B; S3, drying and calcining: the white filter cake B obtained in step S2 is flash dried, calcined and crushed to obtain an iron phosphate material with a high iron-phosphorus ratio.

2. The method for preparing high iron-to-phosphorus ratio ferric phosphate according to claim 1, characterized in that: In the step S1, the mass concentration of the hydrogen peroxide solution is 10-30wt%, the concentration of the ferrous salt solution is 0.5-2.0 mol / L, and the concentration of the phosphate solution is 0.5-2.0 mol / L.

3. The method for preparing high iron-to-phosphorus ratio ferric phosphate according to claim 1, characterized in that: In the step S1, the pH of the synthesis reaction is ≤2.

5.

4. The method for preparing high iron-to-phosphorus ratio ferric phosphate according to claim 1, characterized in that: In step S1, the ferrous salt solution is prepared from any one of ferrous sulfate, ferrous nitrate, ferrous chloride, iron powder, and iron sheet as a raw material; the phosphate salt solution is prepared from any one of ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, and phosphoric acid as a raw material.

5. The method for preparing high iron-to-phosphorus ratio ferric phosphate according to claim 1, characterized in that: In the step S1, the molar ratio of the hydrogen peroxide in the hydrogen peroxide solution to the molar ratio of the iron element in the ferrous salt solution is n(Fe):n(H2O2)=1:0.5-1:

1.

6. The method for preparing high iron-to-phosphorus ratio ferric phosphate according to claim 1, characterized in that: In the step S1, the molar ratio of the phosphorus element in the phosphate salt solution to the iron element in the ferrous salt solution is n(Fe):n(P)=1:0.9-1:1.

2.

7. The method for preparing high iron-to-phosphorus ratio ferric phosphate according to claim 1, characterized in that: In the step S2, after adding the phosphoric acid solution, the pH of the slurry is controlled to be 1.6-2.

0.

8. The method for preparing high iron-to-phosphorus ratio ferric phosphate according to claim 1, characterized in that: In the step S2, the amount of ammonium metavanadate added is n(V):n(Fe)=0.3%-1.5%.

9. The method for preparing high iron-to-phosphorus ratio ferric phosphate according to claim 1, characterized in that: In step S2, the specific method of heating and heat preservation treatment is: heating to 90-100° C. and then keeping the temperature for 2-4 hours.

10. The high iron-phosphorus ratio ferric phosphate prepared by the method for preparing high iron-phosphorus ratio ferric phosphate according to claim 9, characterized in that: The iron-phosphorus ratio of the ferric phosphate is greater than 0.980; the vanadium content in the ferric phosphate is 1500-5000 ppm.

Citation Information

Patent Citations

  • Crystalline iron phosphate doped with metal, method for preparing same, and lithium composite metal phosphate prepared therefrom

    CN104024154A

  • Multiple ions co-doped lithium iron phosphate material and preparation method thereof

    CN105152155A

  • Iron phosphate material with dense sections, preparation method of iron phosphate material and application of iron phosphate material in preparation of lithium iron phosphate

    CN117049491A

  • Method for preparing lithium iron phosphate from hydroxyl ferric phosphate and ferric oxide and application of lithium iron phosphate

    CN117430103A

  • Doped iron phosphate precursor as well as preparation method and application thereof

    CN117842954A