Lithium nickel iron phosphate positive electrode material and preparation method thereof, positive electrode plate and secondary battery

In the preparation of nickel-iron lithium iron phosphate positive electrode material, the mixture and sintering of iron-nickel co-precipitate with lithium source and phosphorus source, combined with doping of transition metals and non-metal elements, the impurity phases in the prior art are solved. Problem, high-performance pure-phase nickel-iron-ferrophosphate cathode material was prepared, which improved its electrochemical performance and energy density.

CN118929608APending Publication Date: 2024-11-12SHENZHEN DYNANONIC CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411001684.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing preparation methods for lithium nickel iron phosphate positive electrode materials have resulted in more impurities in the finished product, which limits the performance of electrochemical properties.

Method used

By dissolving the iron and nickel sources in solution, adding a precipitant dropwise to form an iron and nickel co-precipitate, mixed with the lithium and phosphorus sources, the ball mill is mixed, and then dried, sintered under a protective atmosphere, combining the doping of transition metals and non-metallic elements. To prepare a pure phase nickel-iron-iron phosphate positive electrode material.

Benefits of technology

The preparation of pure phase nickel-iron lithium iron phosphate cathode material is realized, and its electrochemical properties are improved, including cycle stability, electron conductivity and lithium ion diffusion coefficient, thereby improving energy density and processing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929608A_ABST
    Figure CN118929608A_ABST
Patent Text Reader

Abstract

The invention provides a lithium iron nickel phosphate positive electrode material and a preparation method thereof, a positive electrode plate and a secondary battery. The preparation method of the lithium iron nickel phosphate positive electrode material comprises the following steps: dissolving an iron source and a nickel source in a solution to obtain a mixed solution; under a stirring condition, dropwise adding a precipitant into the mixed solution, and reacting to obtain an iron-nickel coprecipitate; mixing the iron-nickel coprecipitate with a lithium source and a phosphorus source, and performing ball milling and drying to obtain precursor powder; and sintering the precursor powder in a protective atmosphere to obtain the lithium iron nickel phosphate positive electrode material. According to the preparation method of the lithium iron nickel phosphate positive electrode material provided by the invention, the pure-phase lithium iron nickel phosphate positive electrode material can be prepared, and the electrochemical performance of the lithium iron nickel phosphate positive electrode material can be favorably exerted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a nickel iron phosphate lithium positive electrode material and a preparation method thereof, a positive electrode plate and a secondary battery. Background Art

[0002] As a high-energy, green and environmentally friendly battery, lithium-ion battery has the advantages of high operating voltage, high energy density, and long cycle life. It is widely used in new energy vehicles, electrochemical energy storage, 3C electronic products and other industries. However, as the market's requirements for lithium-ion batteries continue to increase, finding a higher capacity cathode material is one of the hot issues in the current frontier research field of lithium batteries. As one of the most important factors restricting the performance of lithium batteries, the cathode material of lithium-ion batteries has an extremely important impact on the capacity and cycle life of lithium batteries. Among the cathode materials of lithium-ion batteries, olivine-structured lithium nickel iron phosphate combines the advantages of lithium iron phosphate and lithium nickel phosphate, which can overcome the problems of low energy density of lithium iron phosphate and poor electronic conductivity and low lithium ion diffusion coefficient of lithium nickel phosphate. However, the finished product produced by the existing preparation method of lithium nickel iron phosphate has more impurities, which limits the electrochemical performance of lithium nickel iron phosphate. Summary of the invention

[0003] The present application provides a lithium nickel iron phosphate positive electrode material and a preparation method thereof, a positive electrode plate and a secondary battery, aiming to solve the problem that the lithium nickel iron phosphate positive electrode material prepared by the existing preparation method of the lithium nickel iron phosphate positive electrode material has a large amount of impurity phases.

[0004] In a first aspect, the present application provides a method for preparing a nickel iron phosphate lithium positive electrode material, the method for preparing a nickel iron phosphate lithium positive electrode material comprising:

[0005] dissolving an iron source and a nickel source in a solution to obtain a mixed solution;

[0006] Under stirring conditions, adding a precipitant dropwise to the mixed solution to react and obtain an iron-nickel coprecipitate;

[0007] The iron-nickel coprecipitate is mixed with a lithium source and a phosphorus source, ball-milled, and dried to obtain a precursor powder;

[0008] The precursor powder is sintered under a protective atmosphere to obtain a nickel iron phosphate lithium positive electrode material.

[0009] The method for preparing the lithium nickel iron phosphate positive electrode material provided in the embodiment of the present application can prepare a pure phase lithium nickel iron phosphate positive electrode material, which is beneficial to the electrochemical performance of the lithium nickel iron phosphate positive electrode material.

[0010] In one embodiment, the precursor powder is sintered under a protective atmosphere to obtain a lithium nickel iron phosphate positive electrode material, comprising: sintering the precursor powder under a protective atmosphere to obtain a primary sintering product; mixing the primary sintering product with a carbon source, ball milling, drying, and sintering to obtain the lithium nickel iron phosphate positive electrode material.

[0011] In one embodiment, the iron-nickel co-precipitate is mixed with a lithium source and a phosphorus source, ball-milled, and dried to obtain a precursor powder, comprising: mixing the iron-nickel co-precipitate with a lithium source, a phosphorus source and a transition metal source, ball-milled, and dried to obtain a precursor powder.

[0012] In one embodiment, the transition metal source includes at least one of a titanium source and a magnesium source.

[0013] In one embodiment, the mass ratio of the transition metal element in the transition metal source to the nickel iron phosphate lithium positive electrode material is (0.05% to 0.5%):1.

[0014] In one embodiment, the precursor powder is sintered under a protective atmosphere to obtain a lithium nickel iron phosphate positive electrode material, comprising: sintering the precursor powder under a protective atmosphere to obtain a primary sintering product; mixing the primary sintering product with a non-metallic source, ball milling, drying, and sintering to obtain the lithium nickel iron phosphate positive electrode material.

[0015] In one embodiment, the non-metal source includes at least one of a boron source and a fluorine source.

[0016] In one embodiment, the mass ratio of the non-metallic element in the non-metallic source to the primary sintered product is (0.05% to 0.5%):1.

[0017] In one embodiment, the molar ratio of the iron element in the iron source, the nickel element in the nickel source, the lithium element in the lithium source, and the phosphorus element in the phosphorus source is (0.2-0.8):(0.8-0.2):(1.02-1.05):1.0.

[0018] In one embodiment, the molar ratio of the iron element in the iron source, the nickel element in the nickel source, the lithium element in the lithium source, and the phosphorus element in the phosphorus source is 0.5:0.5:1.02:1.

[0019] In one embodiment, the concentration of the mixed solution is 0.01 mol / L to 2 mol / L.

[0020] In one embodiment, the stirring condition includes a stirring speed of 300 rpm to 900 rpm.

[0021] In one embodiment, the reaction conditions for adding a precipitant to the mixed solution to obtain an iron-nickel co-precipitate include at least one of a reaction temperature of 60° C. to 90° C., a reaction pH of 8 to 10, and a reaction time of 1 h to 5 h.

[0022] In one embodiment, the iron-nickel co-precipitate is mixed with the lithium source and the phosphorus source, and the ball milling speed is 300 rpm to 500 rpm and the ball milling time is 2 h to 6 h.

[0023] In a second aspect, the present application provides a lithium nickel iron phosphate positive electrode material, wherein the lithium nickel iron phosphate positive electrode material is prepared by the preparation method of the lithium nickel iron phosphate positive electrode material as described in any one of the above items.

[0024] In a third aspect, the present application provides a positive electrode plate, which includes a lithium nickel iron phosphate positive electrode material prepared by the preparation method of a lithium nickel iron phosphate positive electrode material as described in any of the above items, or includes the lithium nickel iron phosphate positive electrode material as described above.

[0025] In a fourth aspect, the present application provides a secondary battery, comprising a negative electrode plate, a separator, and the positive electrode plate as described above. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments of the present application will be described below.

[0027] Figure 1 This is the XRD diagram of the lithium nickel iron phosphate positive electrode material prepared in Example 2, Example 5, Example 9 and Comparative Example 1.

[0028] Figure 2 This is the SEM image of the nickel iron phosphate lithium positive electrode material prepared in Example 1.

[0029] Figure 3 This is the SEM image of the nickel iron phosphate lithium positive electrode material prepared in Example 2.

[0030] Figure 4 This is the SEM image of the nickel iron phosphate lithium positive electrode material prepared in Example 3.

[0031] Figure 5 This is the SEM image of the nickel iron phosphate lithium positive electrode material prepared in Example 4.

[0032] Figure 6 This is the SEM image of the nickel iron phosphate lithium positive electrode material prepared in Example 5.

[0033] Figure 7 This is the SEM image of the nickel iron phosphate lithium positive electrode material prepared in Example 9.

[0034] Figure 8 This is the SEM image of the nickel iron phosphate lithium positive electrode material prepared in Comparative Example 1. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.

[0036] Batteries such as lithium-ion secondary batteries usually include a positive electrode, a negative electrode and a separator. The positive electrode is used to provide active lithium ions to the battery, and the negative electrode can be used as a carrier of active lithium ions and electrons during the battery charging and discharging process. The separator is arranged between the positive electrode and the negative electrode to separate the positive electrode and the negative electrode. The separator is used to allow active lithium ions to pass through and block electrons from passing through. The positive electrode includes a positive electrode material, which is used to provide active lithium ions for the lithium-ion battery. The active lithium ions migrate between the positive electrode and the negative electrode of the battery, thereby realizing the battery charging and discharging.

[0037] It is difficult to obtain pure-phase lithium nickel iron phosphate positive electrode material using the existing preparation method of lithium nickel iron phosphate positive electrode material, which affects the electrochemical performance of lithium nickel iron phosphate.

[0038] The present application provides a method for preparing a nickel iron phosphate lithium positive electrode material. The method for preparing a nickel iron phosphate lithium positive electrode material comprises step S1, step S2, step S3 and step S4. The specific steps are as follows:

[0039] Step S1, dissolving an iron source and a nickel source in a solution to obtain a mixed solution;

[0040] Step S2, adding a precipitant dropwise to the mixed solution under stirring to react and obtain an iron-nickel coprecipitate;

[0041] Step S3, mixing the iron-nickel coprecipitate with a lithium source and a phosphorus source, ball milling, and drying to obtain a precursor powder;

[0042] Step S4, sintering the precursor powder under a protective atmosphere to obtain a nickel iron phosphate lithium positive electrode material.

[0043] Wherein, in step S1, the iron source and the nickel source are mixed in the solution, which is conducive to achieving uniform mixing of the iron source and the nickel source at the molecular level. Then, in step S2, an iron-nickel coprecipitate is obtained by coprecipitation reaction. The iron atoms and nickel atoms in the nickel-iron coprecipitate are evenly distributed at the atomic level. In step S3, the iron-nickel coprecipitate is first mixed with a lithium source and a phosphorus source, and then sintered in step S4, which is conducive to the iron-nickel coprecipitate and the lithium source and the phosphorus source fully reacting to obtain a nickel iron phosphate lithium positive electrode material.

[0044] The method for preparing the lithium nickel iron phosphate positive electrode material provided in the embodiment of the present application can prepare a pure phase lithium nickel iron phosphate positive electrode material, which is beneficial to the electrochemical performance of the lithium nickel iron phosphate positive electrode material.

[0045] In one embodiment, step S3 comprises: mixing the iron-nickel coprecipitate with a lithium source, a phosphorus source and a transition metal source, ball milling, and drying to obtain a precursor powder. In step S3, the transition metal source is added and ball milled together, and in the prepared product, the transition metal body is doped in the lithium nickel iron phosphate.

[0046] In the embodiment of the present application, by doping with transition metals, on the one hand, the NiO octahedral structure in the lithium nickel iron phosphate crystal structure can be stabilized to prevent the irreversible collapse of the lithium nickel iron phosphate crystal structure, thereby improving the cycle stability of the lithium nickel iron phosphate positive electrode material. On the other hand, the transition metal element doping produces defects in the lithium nickel iron phosphate crystal structure, improves the intrinsic electronic conductivity and lithium ion diffusion coefficient of the lithium nickel iron phosphate positive electrode material, thereby improving the electrochemical performance of the lithium nickel iron phosphate positive electrode material.

[0047] In one embodiment, the transition metal source includes at least one of a titanium source and a magnesium source. At least one of the titanium element and the magnesium element is doped in the lithium nickel iron phosphate positive electrode material. In the embodiment of the present application, by selecting the doped transition metal, it is beneficial to improve the structural stability and electrochemical performance of the lithium nickel iron phosphate positive electrode material.

[0048] In one embodiment, the mass ratio of the transition metal element in the transition metal source to the lithium nickel iron phosphate positive electrode material is (0.05% to 0.5%): 1. Among them, the relative content of the transition metal element in the transition metal source affects the performance of the lithium nickel iron phosphate positive electrode material. If the content of the transition metal element in the transition metal source is too low, the role of the transition metal element in improving the structural stability and electrochemical performance of the lithium nickel iron phosphate positive electrode material is not obvious. If the content of the transition metal element in the transition metal source is too high, the transition metal element will reduce the energy density of the lithium nickel iron phosphate positive electrode material.

[0049] In the embodiment of the present application, during the preparation process of the lithium nickel iron phosphate positive electrode material, the amount of transition metal source added is controlled to control the doping amount of the transition metal, which improves the structural stability and electrochemical properties of the lithium nickel iron phosphate positive electrode material without increasing the mass of the lithium nickel iron phosphate positive electrode material too much, thereby making the lithium nickel iron phosphate positive electrode material have a higher energy density.

[0050] In one embodiment, the mass ratio of the transition metal element in the transition metal source to the lithium nickel iron phosphate positive electrode material can be 0.05%:1, 0.1%:1, 0.15%:1, 0.2%:1, 0.25%:1, 0.3%:1, 0.35%:1, 0.4%:1, 0.45%:1 or 0.5%:1.

[0051] In one implementation, step S4 includes step S4-1 and step S4-2, and the specific steps are as follows:

[0052] Step S4-1, sintering the precursor powder under a protective atmosphere to obtain a primary sintered product;

[0053] Step S4-2, mixing the primary sintering product with a non-metallic source, ball milling, drying, and sintering to obtain a nickel iron phosphate lithium positive electrode material.

[0054] Wherein, the primary sintered product is lithium nickel iron phosphate. If a transition metal source is added in step S3, the primary sintered product is lithium nickel iron phosphate doped with transition metal elements. The primary sintered product is mixed with a non-metallic source and sintered so that the non-metallic element is doped on the surface of the primary sintered product, namely, lithium nickel iron phosphate. In one embodiment, by controlling the amount of the non-metallic source added, the non-metallic element can be coated on the outer surface of the primary sintered product.

[0055] In the embodiment of the present application, the surface of the lithium nickel iron phosphate positive electrode material is modified so that the surface of the lithium nickel iron phosphate positive electrode material is doped with non-metallic elements. The lithium nickel iron phosphate positive electrode material modified with surface non-metallic elements has a lower pH value, a smaller specific surface area, a higher compaction density, a higher conductivity and a higher lithium ion diffusion coefficient, which is beneficial to improving the processing performance, electrochemical performance and energy density of the lithium nickel iron phosphate positive electrode material.

[0056] In one embodiment, the non-metallic source includes at least one of a boron source and a fluorine source. Among them, at least one of the boron element and the fluorine element is used for surface modification of the lithium nickel iron phosphate positive electrode material. In the embodiment of the present application, by selecting the non-metallic element for surface modification, it is beneficial to improve the processing performance, electrochemical performance and energy density of the lithium nickel iron phosphate positive electrode material.

[0057] In one embodiment, the mass ratio of the non-metallic element in the non-metallic source to the primary sintered product is (0.05% to 0.5%): 1. Among them, the relative content of the non-metallic element in the non-metallic source affects the performance of the lithium nickel iron phosphate positive electrode material. If the content of the non-metallic element in the non-metallic source is too low, the role of the non-metallic element in improving the processing performance and electrochemical performance of the lithium nickel iron phosphate positive electrode material is not obvious. If the content of the non-metallic element in the non-metallic source is too high, the non-metallic element will reduce the energy density of the lithium nickel iron phosphate positive electrode material.

[0058] In the embodiment of the present application, during the preparation process of the lithium nickel iron phosphate positive electrode material, the amount of non-metallic source added is controlled to control the doping amount of the non-metallic element. While improving the processing performance and electrochemical properties of the lithium nickel iron phosphate positive electrode material, the mass of the lithium nickel iron phosphate positive electrode material will not be increased too much, thereby making the lithium nickel iron phosphate positive electrode material have a higher energy density.

[0059] In one embodiment, the mass ratio of the non-metallic element in the non-metallic source to the primary sintered product can be 0.05%:1, 0.1%:1, 0.15%:1, 0.2%:1, 0.25%:1, 0.3%:1, 0.35%:1, 0.4%:1, 0.45%:1 or 0.5%:1.

[0060] In one embodiment, step S4-2 includes: mixing the primary sintered product with a non-metallic source and a carbon source, ball milling, drying, and sintering to obtain a lithium nickel iron phosphate positive electrode material. The carbon source is sintered to form a carbon material. The carbon material has electrical conductivity and can improve the overall electrical conductivity of the lithium nickel iron phosphate positive electrode material.

[0061] In the embodiments of the present application, the surface of the lithium nickel iron phosphate positive electrode material is modified by carbon materials and non-metallic elements, which not only improves the electronic conductivity and lithium ion diffusion coefficient of the lithium nickel iron phosphate positive electrode material, but also improves the processing performance, electrochemical performance and energy density of the lithium nickel iron phosphate positive electrode material.

[0062] In one embodiment, the mass ratio of the primary sintered product, the carbon material, and the non-metallic element in the non-metallic source is 1:(0.05-0.2):(0.05%-0.5%).

[0063] In one embodiment, the amount of carbon source added is controlled so that the carbon material forms a coating layer that covers the outer surface of the primary sintered product. The formation of the coating layer is conducive to increasing the binding force between the carbon material and the non-metallic element and the primary sintered product, and the carbon material and the non-metallic element are not easy to fall off, which is conducive to their role in improving the performance of the nickel iron phosphate lithium positive electrode material.

[0064] In one implementation, step S4 includes step S4-1' and step S4-2', and the specific steps are as follows:

[0065] Step S4-1', sintering the precursor powder under a protective atmosphere to obtain a primary sintered product;

[0066] Step S4-2', mixing the primary sintered product with a carbon source, ball milling, drying, and sintering to obtain a lithium nickel iron phosphate positive electrode material.

[0067] The primary sintered product is mixed with a carbon source and sintered, so that the carbon material is bonded to the surface of the primary sintered product, namely, lithium nickel iron phosphate.

[0068] In the embodiment of the present application, the surface of the lithium nickel iron phosphate positive electrode material is modified so that the surface of the lithium nickel iron phosphate positive electrode material is combined with a carbon material. The lithium nickel iron phosphate positive electrode material modified with the surface carbon material has a higher electrical conductivity and a higher lithium ion diffusion coefficient.

[0069] In one embodiment, the mass ratio of the primary sintering product to the carbon material is 1:(0.05-0.2). In the embodiment of the present application, by controlling the amount of carbon material added, while improving the conductivity and lithium ion diffusion coefficient of the lithium nickel iron phosphate positive electrode material, the mass of the lithium nickel iron phosphate positive electrode material will not be increased too much, so that the lithium nickel iron phosphate positive electrode material has a higher energy density.

[0070] In one embodiment, in step S4-2', the ball milling speed of the primary sintered product and the carbon material is 300 rpm to 500 rpm and the ball milling time is 2 h to 6 h.

[0071] In one embodiment, the molar ratio of the iron element in the iron source, the nickel element in the nickel source, the lithium element in the lithium source, and the phosphorus element in the phosphorus source is (0.2-0.8):(0.8-0.2):(1.02-1.05):1.0.

[0072] In one embodiment, the molar ratio of the iron element in the iron source, the nickel element in the nickel source, the lithium element in the lithium source, and the phosphorus element in the phosphorus source can be 0.2:0.8:1.02:1.0, 0.3:0.7:1.025:1.0, 0.4:0.6:1.03:1.0, 0.5:0.5:1.04:1.0, 0.6:0.4:1.05:1.0, 0.7:0.3:1.025:1.0 or 0.8:0.2:1.035:1.0.

[0073] Preferably, the molar ratio of the iron element in the iron source, the nickel element in the nickel source, the lithium element in the lithium source, and the phosphorus element in the phosphorus source is 0.5:0.5:1.02:1.0. The chemical formula of the prepared lithium nickel iron phosphate positive electrode material is LiFe 0.5 Ni 0.5 PO4.

[0074] In one embodiment, the concentration of the mixed solution is 0.01 mol / L to 2 mol / L. In the embodiment of the present application, by controlling the concentration of the mixed solution in step S1, it is beneficial to mix the iron element and the nickel element evenly, and it is beneficial to the subsequent coprecipitation reaction, so as to obtain a pure phase of nickel iron phosphate lithium positive electrode material.

[0075] In one embodiment, the concentration of the mixed solution can be 0.01mol / L, 0.1mol / L, 0.2mol / L, 0.3mol / L, 0.4mol / L, 0.5mol / L, 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L, 1mol / L, 1.1mol / L, 1.2mol / L, 1.3mol / L, 1.4mol / L, 1.5mol / L, 1.6mol / L, 1.7mol / L, 1.8mol / L, 1.9mol / L or 2mol / L.

[0076] In one embodiment, the stirring condition includes a stirring speed of 300 rpm to 900 rpm. In the present embodiment, by controlling the stirring speed in step S2 within an appropriate range, it is more conducive to the coprecipitation reaction and to obtaining an iron-nickel coprecipitate with a moderate particle size and a better morphology.

[0077] In one embodiment, a precipitant is added to the mixed solution, and the reaction conditions for obtaining the iron-nickel coprecipitate include at least one of a reaction temperature of 60°C to 90°C, a reaction pH of 8 to 10, and a reaction time of 1h to 5h. Wherein, the reaction temperature between the mixed solution and the precipitant can be controlled by heating in a water bath, and at this time, the reaction temperature is the temperature of the water bath heating. Due to the coprecipitation reaction, the pH value in the mixed solution will change. At this time, by regulating the pH value in the mixed solution, it is beneficial to continue the coprecipitation reaction, so that the nickel ions and iron ions form the iron-nickel coprecipitate as much as possible.

[0078] In the embodiments of the present application, by controlling the reaction conditions of the coprecipitation reaction, it is more conducive to the coprecipitation reaction and is more conducive to obtaining an iron-nickel coprecipitate with a moderate particle size and a better morphology.

[0079] In one embodiment, the iron-nickel coprecipitate is mixed with a lithium source and a phosphorus source, and the ball milling speed is 300 rpm to 500 rpm and the ball milling time is 2 h to 6 h. In the embodiment of the present application, the iron-nickel coprecipitate is ball milled with a lithium source and a phosphorus source at a lower speed, which is more conducive to uniform mixing of the iron-nickel coprecipitate with the lithium source and the phosphorus source, so as to facilitate subsequent sintering to form a pure phase of nickel iron phosphate lithium positive electrode material.

[0080] In one embodiment, the iron source includes at least one of ferric chloride, ferric sulfate, ferric nitrate, ferric acetate, ferric phosphate, ferrous sulfate, ferrous phosphate, and ferrous oxalate.

[0081] In one embodiment, the nickel source includes at least one of nickel chloride, nickel sulfate, nickel nitrate, nickel acetate, and nickel oxalate.

[0082] In one embodiment, the precipitant includes at least one of aqueous ammonia, sodium hydroxide, and potassium hydroxide.

[0083] In one embodiment, the lithium source includes at least one of lithium chloride, lithium nitrate, lithium oxalate, lithium acetate, and lithium phosphate.

[0084] In one embodiment, the phosphorus source includes at least one of phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, iron phosphate, and lithium phosphate.

[0085] In one embodiment, the carbon source includes at least one of glucose, sucrose, starch, polyvinyl alcohol, polyethylene glycol, citric acid, and graphene.

[0086] In one embodiment, the non-metallic element source includes at least one of boron trioxide, boric acid, hexafluoroboric acid, borax, borane, ammonium fluoride, hexafluoroboric acid, and lithium fluoride.

[0087] In one embodiment, the transition metal source comprises a titanium source, and the titanium source comprises titanium oxide, titanium tetrachloride.

[0088] In one embodiment, the transition metal source includes a magnesium source, and the magnesium source includes at least one of magnesium oxide, magnesium chloride, magnesium sulfate, magnesium nitrate, magnesium acetate, and magnesium nitrate.

[0089] In one embodiment, the protective atmosphere in step S4 includes at least one of nitrogen and argon.

[0090] In one embodiment, sintering the precursor powder in step S4 includes: heating the precursor powder to a first sintering temperature at a heating rate of 2°C / min to 10°C / min, and keeping the temperature at the first sintering temperature for 1h to 6h; and then keeping the temperature at a second sintering temperature for 3h to 10h. The first sintering temperature is a temperature between 300°C and 500°C, and the second sintering temperature is a temperature between 650°C and 800°C.

[0091] The present application provides a nickel iron phosphate lithium positive electrode material, wherein the nickel iron phosphate lithium positive electrode material is prepared by the preparation method of the nickel iron phosphate lithium positive electrode material as described above.

[0092] The present application provides a positive electrode plate, which includes the lithium nickel iron phosphate positive electrode material as described above, or includes the lithium nickel iron phosphate positive electrode material prepared by the preparation method of the lithium nickel iron phosphate positive electrode material as described above.

[0093] The present application provides a secondary battery, which includes a negative electrode plate, a separator and the positive electrode plate as described above.

[0094] In order to illustrate the beneficial effects of the method of the present application, the present application also provides the following examples and comparative examples:

[0095] Example 1

[0096] Embodiment 1 provides a method for preparing a nickel iron phosphate lithium positive electrode material, comprising:

[0097] Step 1: weigh ferrous sulfate and nickel sulfate at a molar ratio of Fe:Ni=1:1 and dissolve them in deionized water to obtain Fe 2+ / Ni 2+ The metal ion mixed solution ensures that the total metal ion concentration in the mixed solution is 0.5 mol / L.

[0098] Step 2: Add concentrated ammonia solution dropwise to the mixed solution at 90°C in a water bath and 400rpm magnetic stirring to maintain the pH value of the solution at 9 to make the divalent Fe 2+ and Ni 2+ The ions coprecipitate. At this temperature and under constant stirring, the reaction is maintained for 2.5 hours. After the reaction is completed, the coprecipitate is filtered and washed with deionized water, and the process is repeated three times. Then, it is placed in a vacuum oven at 80°C and dried for 24 hours to obtain an iron-nickel coprecipitate.

[0099] Step three, weigh the prepared iron-nickel co-precipitate, lithium hydroxide and ammonium dihydrogen phosphate to ensure that the molar ratio of (Fe+Ni):Li:P is 1:1.02:1; then place the weighed materials in a ball mill, and ball mill them at 400 rpm in an ethanol medium for 4 hours; finally, transfer them to a vacuum oven at 100°C and dry them for 24 hours, and crush them through a 200-mesh sieve to obtain a fine precursor powder.

[0100] Step 4: Place the precursor powder in a tube furnace, and under the protection of N2 atmosphere, first heat it to 500°C at a heating rate of 5°C / min, keep it warm for 2 hours, then heat it to 750°C at a heating rate of 5°C / min, keep it warm for 6 hours, and naturally cool it to room temperature to obtain an unmodified pure phase lithium iron nickel phosphate positive electrode material, denoted as LiFe 0.5 Ni 0.5 PO4.

[0101] Example 2

[0102] Embodiment 2 provides a method for preparing a nickel iron phosphate lithium positive electrode material, which is different from Embodiment 1 in that Embodiment 2 further includes:

[0103] The prepared LiFe 0.5 Ni 0.5 PO4 and glucose were added into a ball mill at a mass ratio of 1:0.1, and ball milled at 400 rpm for 4 hours in an ethanol medium. Finally, the ball milled ...

[0104] The modified powder was placed in a tube furnace, and under the protection of N2 atmosphere, the temperature was raised to 700°C at a rate of 5°C / min, kept at this temperature for 2 hours, and naturally cooled to room temperature to obtain a surface carbon-coated modified lithium iron nickel phosphate positive electrode material, denoted as LiFe 0.5 Ni 0.5 PO4 / C.

[0105] Example 3

[0106] Example 3 provides a method for preparing a nickel iron phosphate lithium positive electrode material, which is different from Example 2 in that, in Example 3, LiFe 0.5 Ni 0.5 The mass ratio of PO4 to glucose is 1:0.15, and the obtained surface carbon-coated modified lithium iron phosphate cathode material is denoted as LiFe 0.5 Ni 0.5 PO4 / C15.

[0107] Example 4

[0108] Example 4 provides a method for preparing a nickel iron phosphate lithium positive electrode material, which is different from Example 2 in that, in Example 3, LiFe 0.5 Ni 0.5 The mass ratio of PO4 to glucose is 1:0.2, and the obtained surface carbon-coated modified lithium iron phosphate cathode material is denoted as LiFe 0.5 Ni 0.5 PO4 / C20.

[0109] Example 5

[0110] Example 5 provides a method for preparing a nickel iron phosphate lithium positive electrode material, which is different from Example 1 in that Example 5 also includes:

[0111] The prepared LiFe 0.5 Ni 0.5 PO4, glucose and boron trioxide are added to the ball mill in a certain mass ratio to ensure that LiFe 0.5 Ni 0.5 The mass ratio of PO4: glucose: B element is 1: 0.1: 0.15%. It is ball-milled at 400 rpm in an ethanol medium for 4 hours, and finally transferred to a vacuum oven at 100° C. for drying for 24 hours. It is crushed through a 200-mesh sieve to obtain fine modified powder.

[0112] The modified powder was placed in a tube furnace, and under the protection of N2 atmosphere, the temperature was raised to 700°C at a rate of 5°C / min, kept at this temperature for 2 hours, and naturally cooled to room temperature to obtain a surface-modified lithium iron nickel phosphate positive electrode material, denoted as LiFe 0.5 Ni 0.5PO4-B / C.

[0113] Example 6

[0114] Example 6 provides a method for preparing a nickel iron phosphate lithium positive electrode material. The difference from Example 1 is that in Example 6, the boron trioxide in Example 5 is replaced by ammonium fluoride, and the surface-modified nickel iron phosphate lithium positive electrode material obtained is recorded as LiFe 0.5 Ni 0.5 PO4-F / C.

[0115] Example 7

[0116] Embodiment 7 provides a method for preparing a nickel iron phosphate lithium positive electrode material, comprising:

[0117] Step 1: weigh ferrous sulfate and nickel sulfate at a molar ratio of Fe:Ni=1:1 and dissolve them in deionized water to obtain Fe 2+ / Ni 2+ The metal ion mixed solution ensures that the total metal ion concentration in the mixed solution is 0.5 mol / L.

[0118] Step 2: Add concentrated ammonia solution dropwise to the mixed solution at 90°C in a water bath and 400rpm magnetic stirring to maintain the pH value of the solution at 9 to make the divalent Fe 2+ and Ni 2+ The ions coprecipitate. At this temperature and under constant stirring, the reaction is maintained for 2.5 hours. After the reaction is completed, the coprecipitate is filtered and washed with deionized water, and the process is repeated three times. Then, it is placed in a vacuum oven at 80°C and dried for 24 hours to obtain an iron-nickel coprecipitate.

[0119] Step 3, weigh the prepared coprecipitate, lithium hydroxide, ammonium dihydrogen phosphate and titanium chloride to ensure that the molar ratio of (Fe+Ni): Li: P: Ti is 0.97: 1.02: 1: 0.4; then place the weighed materials in a ball mill, and ball mill them at 400 rpm in an ethanol medium for 4 hours; finally, transfer them to a vacuum oven at 100° C. and dry them for 24 hours, and crush them through a 200-mesh sieve to obtain fine transition metal Ti-doped LiFe 0.5 Ni 0.5 PO4 precursor powder.

[0120] Step 4: Place the precursor powder in a tube furnace, and under the protection of N2 atmosphere, first increase the temperature to 500°C at a heating rate of 5°C / min, keep it warm for 2 hours, then increase the temperature to 750°C at a heating rate of 5°C / min, keep it warm for 6 hours, and naturally cool to room temperature to obtain a pure phase lithium iron nickel phosphate positive electrode material doped with transition metal Ti element, recorded as Ti-LiFe 0.5 Ni 0.5 PO4.

[0121] The prepared Ti-LiFe 0.5 Ni 0.5 PO4, glucose and boron oxide are added to the ball mill in a certain mass ratio to ensure that LiFe 0.5 Ni 0.5 The mass ratio of PO4: glucose: B element is 1: 0.1: 0.15%. It is ball-milled at 400 rpm in an ethanol medium for 4 hours, and finally transferred to a vacuum oven at 100° C. for drying for 24 hours. It is crushed through a 200-mesh sieve to obtain fine modified powder.

[0122] The modified powder was placed in a tube furnace, and under the protection of N2 atmosphere, the temperature was raised to 700℃ at a rate of 5℃ / min, kept at this temperature for 2 hours, and naturally cooled to room temperature to obtain a surface carbon-coated and Ti-doped modified lithium iron phosphate cathode material, which was recorded as Ti-LiFe 0.5 Ni 0.5 PO4-B / C.

[0123] Example 8

[0124] Example 8 provides a method for preparing a nickel-iron-phosphate lithium positive electrode material. The difference from Example 7 is that in Example 8, the titanium source titanium chloride in Example 7 is replaced by magnesium source magnesium sulfate, and the obtained nickel-iron-phosphate lithium positive electrode material is recorded as Mg-LiFe 0.5 Ni 0.5 PO4-B / C.

[0125] Example 9

[0126] Example 8 provides a method for preparing a nickel iron phosphate lithium positive electrode material, which is different from Example 7 in that the titanium source in Example 7 is replaced by two mixed titanium chlorides and magnesium sulfate, and the boron oxide in Example 7 is replaced by hexafluoroboric acid in Example 9. The obtained nickel iron phosphate lithium positive electrode material is recorded as TM-LiFe 0.5 Ni 0.5 PO4-BF / C.

[0127] Comparative Example 1

[0128] Comparative Example 1 provides a method for preparing a nickel iron phosphate lithium positive electrode material, which is different from Example 1 in that, in Comparative Example 1, the nickel iron phosphate lithium positive electrode material is synthesized by a solid phase method, and the method for preparing the nickel iron phosphate lithium positive electrode material includes:

[0129] Ferrous sulfate, nickel sulfate and ammonium dihydrogen phosphate are weighed at a molar ratio of Fe:Ni:P=1:1:2, mixed and ball-milled, and heated to obtain a nickel iron phosphate precursor; the nickel iron phosphate precursor is mixed with lithium hydroxide to ensure that the Li:P molar ratio is 1.02:1, and secondary sintering is performed to obtain a nickel iron phosphate lithium positive electrode material.

[0130] The lithium nickel iron phosphate positive electrode materials provided in the above examples and comparative examples are respectively assembled into positive electrode sheets and lithium ion batteries according to the following methods:

[0131] The positive electrode sheet was prepared as follows: LNFP (LFP): SP: PVDF: NMP = 93.5: 2.5: 4: 100 by mass ratio, and the mixture was stirred at 360 rpm for 1 hour to obtain a positive electrode slurry. The prepared positive electrode slurry was poured on aluminum foil and evenly scraped with a scraper. The positive electrode sheet was dried in an oven at 120°C for 20 minutes, and then rolled at a pressure of 10 MPa to obtain a rolled electrode sheet. A sheet punching machine was used to cut a 12 mm diameter disc in the middle area of ​​the electrode sheet, and the disc was weighed and the thickness was measured to calculate the compaction density.

[0132] The battery assembly process is as follows: the prepared positive electrode plate is attached to the positive electrode metal shell with conductive adhesive and then dried; the metal lithium sheet is used as the negative electrode, the Celgard2400 microporous membrane is used as the battery separator, and a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) containing 1.0M LiPF6 is used as the electrolyte (EC / DEC volume ratio is 1:1), and the button battery is assembled in a glove box.

[0133] Related performance tests

[0134] Cathode material performance test:

[0135] The carbon content was tested using a CS3500 carbon-sulfur analyzer;

[0136] The resistivity is tested using PPMS-resistivity test instrument;

[0137] The average particle size (d) was measured using a scanning electron microscope (SEM) instrument to characterize the material particle morphology and obtain the particle size distribution statistically.

[0138] Electrochemical performance test:

[0139] The electrochemical performance of the button cell was tested using a LAND electrochemical tester, with a charge termination voltage of 3.75 V and a discharge termination voltage of 2.0 V. The obtained lithium-ion battery was subjected to the following performance tests: The button cell was subjected to 0.1C and 1C rate charge and discharge tests at 25°C.

[0140] The relevant performance test results are shown in Table 1 below:

[0141] Table 1 Performance test results

[0142]

[0143] Related spectra characterization Figures 1 to 8 shown. Figure 1 In the figure, the horizontal axis is the 2theta angle of the nickel iron phosphate lithium positive electrode material, that is, 2θ, and the vertical axis is the intensity of the diffraction. Figure 1 It can be seen that the diffraction peaks of Example 2, Example 5, and Example 9 are between pure phase LiFePO4 and pure phase LiNiPO4, and are single components. 0.34 Ni 0.66 The diffraction peaks of PO4 are basically corresponding, with only a shift in the peak position, proving that its crystal structure is a pure phase lithium nickel iron phosphate solid solution. After carbon coating / non-metallic element doping and transition metal element modification, the diffraction peaks have no peaks of other impurities, proving that the modification will not change the crystal structure of pure phase lithium nickel iron phosphate, while the XRD peaks of comparative example 1 show lithium phosphate and nickel phosphide (Ni x P y ) impurity peaks, and no pure phase material was prepared.

[0144] Figure 2 It can be observed that the overall morphology of the particles is a regular polyhedral structure. Due to the lack of protection of the carbon layer, the particle size of the lithium nickel iron phosphate positive electrode material is relatively large, and serious particle agglomeration and adhesion occur, which is not conducive to the infiltration of the electrolyte and the transmission and diffusion of lithium ions, thereby affecting its capacity release.

[0145] Figure 3 It can be observed that the overall morphology of the nickel iron phosphate lithium cathode material particles is spherical. Due to the protective effect of the carbon layer, the growth and agglomeration of the particles are inhibited, and the particle size is significantly reduced compared to that before modification, which is conducive to the infiltration of the electrolyte and the transmission and diffusion of lithium ions, thereby promoting the release of its capacity.

[0146] Depend on Figure 4 It can be seen that the increase in carbon content makes the particles of nickel iron phosphate lithium positive electrode material further reduced, and there are a large number of small particles. This is conducive to the infiltration of electrolyte and the transmission and diffusion of lithium ions, thereby promoting the release of its capacity.

[0147] Depend on Figure 5 It can be seen that further increasing the carbon content can further reduce the size of the nickel iron phosphate lithium cathode material particles, and there are a large number of small particles, but the particles are bonded, which is attributed to the excessive carbon content. This is not conducive to the infiltration of the electrolyte and the transmission and diffusion of lithium ions.

[0148] Figure 6It can be observed that the coexistence and matching of large and small particles of nickel iron phosphate cathode material can improve the compaction density of the material. The grading of large and small particles is conducive to the infiltration of electrolyte and the transmission and diffusion of lithium ions.

[0149] Figure 7 It can be observed that the lithium nickel iron phosphate positive electrode material has the same size particles coexisting and matching, which can not only improve the compaction density of the lithium nickel iron phosphate positive electrode material, but also the size particle grading is beneficial to the infiltration of the electrolyte and the transmission and diffusion of lithium ions. In addition, the bulk doping of transition metal elements is beneficial to improving the electronic conductivity and lithium ion diffusion rate of the lithium nickel iron phosphate positive electrode material and the structural stability of the NiO octahedron.

[0150] Figure 8 It can be observed that the particles of Comparative Example 1 have irregular morphology, poor sphericity, severe particle agglomeration and bonding, and the overall particles are relatively large, which is not conducive to the infiltration of the electrolyte and the transmission and diffusion of lithium ions, thereby affecting the release of its capacity.

[0151] In summary, the finished lithium nickel iron phosphate product prepared by the preparation method of the present application is pure phase LiNiPO4, and the electrochemical performance of the prepared lithium nickel iron phosphate can be further improved by carbon coating and / or non-metallic element modification and / or transition metal element modification.

[0152] The above is a detailed introduction to the lithium nickel iron phosphate positive electrode material and its preparation method, positive electrode plate and secondary battery provided in the embodiments of the present application. Specific examples are used in this article to illustrate the principles and embodiments of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for general technical personnel in this field, according to the ideas of the present application, there will be changes in the specific embodiments and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for preparing a nickel iron phosphate lithium positive electrode material, characterized in that: The preparation method of the nickel iron phosphate lithium positive electrode material comprises: dissolving an iron source and a nickel source in a solution to obtain a mixed solution; Under stirring conditions, adding a precipitant dropwise to the mixed solution to react and obtain an iron-nickel coprecipitate; The iron-nickel coprecipitate is mixed with a lithium source and a phosphorus source, ball-milled, and dried to obtain a precursor powder; The precursor powder is sintered under a protective atmosphere to obtain a nickel iron phosphate lithium positive electrode material.

2. The method for preparing the lithium nickel iron phosphate positive electrode material according to claim 1, characterized in that: The method of sintering the precursor powder under a protective atmosphere to obtain a lithium nickel iron phosphate positive electrode material comprises: sintering the precursor powder under a protective atmosphere to obtain a primary sintered product; The primary sintered product is mixed with a carbon source and ball-milled, and then dried and sintered to obtain a nickel iron phosphate lithium positive electrode material.

3. The method for preparing the lithium nickel iron phosphate positive electrode material according to claim 1 or 2, characterized in that: The iron-nickel coprecipitate is mixed with a lithium source and a phosphorus source, ball-milled, and dried to obtain a precursor powder, comprising: The iron-nickel coprecipitate is mixed with a lithium source, a phosphorus source and a transition metal source, ball-milled and dried to obtain a precursor powder.

4. The method for preparing the lithium nickel iron phosphate positive electrode material according to claim 3, characterized in that: The transition metal source includes at least one of a titanium source and a magnesium source; The mass ratio of the transition metal element in the transition metal source to the nickel iron phosphate lithium positive electrode material is (0.05% to 0.5%):

1.

5. The method for preparing the lithium nickel iron phosphate positive electrode material according to any one of claims 1 to 4, characterized in that: The method of sintering the precursor powder under a protective atmosphere to obtain a lithium nickel iron phosphate positive electrode material comprises: sintering the precursor powder under a protective atmosphere to obtain a primary sintered product; The primary sintering product is mixed with a non-metallic source, ball-milled, dried, and sintered to obtain a nickel iron phosphate lithium positive electrode material.

6. The method for preparing the nickel iron phosphate lithium positive electrode material according to claim 5, characterized in that: The non-metal source includes at least one of a boron source and a fluorine source; and / or The mass ratio of the non-metallic element in the non-metallic source to the primary sintered product is (0.05% to 0.5%):

1.

7. The method for preparing the nickel iron phosphate lithium positive electrode material according to claim 1, characterized in that: The molar ratio of the iron element in the iron source, the nickel element in the nickel source, the lithium element in the lithium source, and the phosphorus element in the phosphorus source is (0.2-0.8):(0.8-0.2):(1.02-1.05):1.0, preferably 0.5:0.5:1.02:1, and / or The concentration of the mixed solution is 0.01 mol / L to 2 mol / L; and / or The stirring conditions include a stirring speed of 300 rpm to 900 rpm; and / or The reaction conditions for adding a precipitant to the mixed solution to obtain an iron-nickel coprecipitate include at least one of a reaction temperature of 60° C. to 90° C., a reaction pH of 8 to 10, and a reaction time of 1 h to 5 h; and / or The iron-nickel coprecipitate is mixed with the lithium source and the phosphorus source, and the ball milling speed is 300 rpm to 500 rpm and the ball milling time is 2 h to 6 h.

8. A nickel iron lithium phosphate positive electrode material, characterized in that: The lithium nickel iron phosphate positive electrode material is prepared by the method for preparing the lithium nickel iron phosphate positive electrode material according to any one of claims 1 to 7.

9. A positive electrode sheet, characterized in that: The positive electrode plate includes a lithium nickel iron phosphate positive electrode material prepared by the method for preparing a lithium nickel iron phosphate positive electrode material as described in any one of claims 1 to 7, or includes a lithium nickel iron phosphate positive electrode material as described in claim 8.

10. A secondary battery, characterized in that: The secondary battery comprises a negative electrode sheet, a separator and the positive electrode sheet as claimed in claim 9.

Citation Information

Patent Citations

  • Method for preparing high-value material by recycling waste ferro-nickel alloy

    CN114592128A

  • Electrode-active anion-deficient lithium transition-metal phosphate, method for preparing the same, and electrochemical device using the same

    KR1020110085600A

  • Anode material precursor, anode material, method for preparing same, and use thereof

    WO2023246724A1