Hard carbon material, preparation method thereof and sodium ion battery

By introducing doping elements into biomass hard carbon materials and using specific cultivation environments and treatment methods, the problem of insufficient electrochemical performance of biomass hard carbon materials is solved, and the electrochemical performance of sodium ion batteries is significantly improved.

CN118929621APending Publication Date: 2024-11-12REPT BATTERO ENERGY CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410970391.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The electrochemical performance of biomass hard carbon materials in sodium ion batteries is insufficient, and the first Coulomb efficiency and reversible specific capacity are not ideal, making it difficult to meet performance requirements.

Method used

By introducing doped elements, such as nitrogen, phosphorus, sulfur, and boron, a hard carbon material containing doped elements is prepared using specific cultivation environments and treatment methods to increase the active site and electrochemical properties of the material.

Benefits of technology

It significantly improves the electrochemical performance of hard carbon materials, improves the sodium storage and electrochemical performance of sodium ion batteries, and achieves higher first-time charging specific capacity, first-time discharge specific capacity and first-time Coulomb efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929621A_ABST
    Figure CN118929621A_ABST
Patent Text Reader

Abstract

The invention relates to a hard carbon material and a preparation method thereof, and a sodium ion battery, the preparation method of the hard carbon material comprises: providing a plant biomass and a doping source containing a doping element, the doping element comprising a non-metallic element; placing the plant biomass in a cultivation environment formed by the doping source for cultivation treatment; and preparing the hard carbon material containing doping elements by taking the cultivated plant biomass as a precursor raw material. The plant biomass is cultivated in the cultivation environment formed by the doping source, the hard carbon material containing the doping element is prepared from the cultivated plant biomass, and the electrochemical performance of the hard carbon material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a hard carbon material and a preparation method thereof, and a sodium ion battery. Background Art

[0002] Among the current sodium energy storage negative electrode materials, hard carbon (HC) materials are hot candidates for negative electrode materials for sodium ion batteries due to their disordered structure, large interlayer spacing, and the ability to quickly embed and extract sodium ions. Among them, biomass hard carbon has attracted much attention due to its wide sources, low cost, and environmental friendliness. However, due to the differences in the characteristics of biomass itself, the specific capacity and first coulombic efficiency of hard carbon materials obtained by direct carbonization are often limited, making it difficult to meet the performance requirements of sodium ion batteries. In order to improve the electrochemical properties of biomass hard carbon materials, the modification methods currently used by researchers include activating the bulk phase of hard carbon and optimizing the material preparation process, but the first coulombic efficiency and reversible specific capacity of biomass hard carbon materials are still not ideal.

[0003] Therefore, how to modify the hard carbon negative electrode material so that it has good electrical properties is a problem that needs to be solved at present. Summary of the invention

[0004] Based on this, it is necessary to provide a hard carbon material and a preparation method thereof, and a sodium ion battery that can improve the electrochemical properties of the hard carbon material.

[0005] One aspect of the present invention provides a method for preparing a hard carbon material, the method comprising:

[0006] Providing plant biomass and a doping source containing a doping element, wherein the doping element includes a non-metallic element;

[0007] placing the plant biomass in a cultivation environment formed by a doping source for cultivation treatment;

[0008] The cultivated plant biomass is used as a precursor raw material to prepare a hard carbon material containing doping elements.

[0009] Optionally, the non-metallic element includes one or more of nitrogen, phosphorus, sulfur or boron.

[0010] Optionally, the method satisfies at least one of the following conditions:

[0011] (1) The doping element includes nitrogen, and the doping source includes one or more of urea, thiourea, diammonium hydrogen phosphate or ammonium pentaborate tetrahydrate;

[0012] (2) the doping element includes phosphorus, and the doping source includes one or more of diammonium hydrogen phosphate or ammonium dihydrogen phosphate;

[0013] (3) The doping element includes sulfur, and the doping source includes thiourea;

[0014] (4) The doping element includes boron, and the doping source includes ammonium pentaborate tetrahydrate.

[0015] Optionally, the cultivation process satisfies at least one of the following conditions:

[0016] (1) The total mass concentration of nitrogen, sulfur, phosphorus and boron in the cultivation environment is (37.18-186) mg / L, and the mass concentration ratio of nitrogen, sulfur, phosphorus and boron is (15.8-79) mg / L: (10.55-52.75) mg / L: (5.86-29.3) mg / L: (4.97-24.8) mg / L;

[0017] (2) The total mass concentration of the nitrogen element, the sulfur element and the phosphorus element in the cultivation environment is (30.91-155) mg / L, and the mass concentration ratio of the nitrogen element, the sulfur element and the phosphorus element is (14.5-72.5) mg / L: (10.55-52.75) mg / L: (5.86-29.3) mg / L;

[0018] (3) The total mass concentration of the nitrogen element, the sulfur element and the boron element in the cultivation environment is (26.02-130) mg / L, and the mass concentration ratio of the nitrogen element, the sulfur element and the boron element is (10.5-52.5) ​​mg / L: (10.55-52.75) mg / L: (4.97-24.8) mg / L.

[0019] Optionally, the cultivation process satisfies at least one of the following conditions:

[0020] (1) The doping source comprises thiourea, diammonium hydrogen phosphate and ammonium pentaborate tetrahydrate; the mass concentration ratio of the thiourea, the diammonium hydrogen phosphate and the ammonium pentaborate tetrahydrate is (25-125) mg / L: (25-125) mg / L: (25-125) mg / L;

[0021] (2) The doping source comprises thiourea and diammonium phosphate; the mass concentration ratio of the thiourea to the diammonium phosphate is (25-125) mg / L: (25-125) mg / L;

[0022] (3) The doping source comprises thiourea and ammonium pentaborate tetrahydrate; the mass concentration ratio of the thiourea to the ammonium pentaborate tetrahydrate is (25-125) mg / L: (25-125) mg / L.

[0023] Optionally, the step of using the cultivated plant biomass as a precursor raw material to prepare a hard carbon material containing doping elements comprises:

[0024] The precursor raw material is washed and dried and then crushed to obtain a first precursor;

[0025] Using an alkaline solution to perform alkaline treatment on the first precursor to obtain a second precursor;

[0026] Carrying out a carbonization treatment on the second precursor to obtain a third precursor;

[0027] The third precursor is subjected to a secondary carbonization treatment to obtain the hard carbon material containing the doping element, wherein the temperature of the primary carbonization treatment is lower than the temperature of the secondary carbonization treatment.

[0028] Optionally, the step of obtaining the hard carbon material containing the doping element satisfies at least one of the following conditions:

[0029] (1) The particle size of the first precursor is 1 μm-12 μm;

[0030] (2) treating the first precursor with an alkaline solution to obtain the second precursor comprises dispersing the first precursor in an alkaline solution to obtain a suspension, stirring at room temperature, washing with deionized water for multiple times until the pH value of the suspension is neutral, and filtering and drying to obtain the second precursor;

[0031] (3) The temperature of the primary carbonization treatment is 500° C.-800° C.;

[0032] (4) The time of the primary carbonization treatment is 1h-6h;

[0033] (5) The temperature of the secondary carbonization treatment is 1000° C.-1500° C.;

[0034] (6) The time of the secondary carbonization treatment is 1h-6h.

[0035] Optionally, the plant biomass includes one or more of Eichhornia crassipes, Ceratophyllum nobile, Phragmites australis or Vallisneria vallisneria.

[0036] The second aspect of the present invention provides a hard carbon material, which is prepared by the preparation method described in the first aspect of the present application.

[0037] The third aspect of the present invention provides a sodium ion battery, comprising the hard carbon material prepared by the preparation method described in the first aspect of the present application or the hard carbon material described in the second aspect of the present application.

[0038] The above-mentioned hard carbon material and its preparation method, and sodium ion battery cultivate and treat plant biomass in a cultivation environment formed by a doping source, and use the cultivated plant biomass to prepare a hard carbon material containing doping elements. The doping elements in the doping source can be adsorbed into the plant biomass through the bioaccumulation of the plant biomass during the cultivation process. The preparation process is simple and easy, and the in-situ combination of the doping elements and the plant biomass material is realized. The hard carbon material prepared by the above method can provide more active sites, improve the sodium storage performance, and achieve the improvement of the electrochemical performance of the hard carbon material. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 Schematic diagram of a method for preparing a hard carbon material according to one embodiment. DETAILED DESCRIPTION

[0040] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0041] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.

[0042] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0043] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0044] If there is no special description, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. If there is no special description, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.

[0045] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, it is mentioned that the method may also include step (c), which means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0046] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0047] Sodium-ion batteries (SIBs) are considered as a potential light metal ion battery due to the abundant reserves of sodium resources, low price and similar chemical properties to lithium. However, since sodium ions have a larger radius than lithium ions, sodium ions are difficult to embed or extract from traditional lithium-ion battery negative electrode materials, so developing a negative electrode material with excellent performance is still one of the challenges of sodium-ion batteries.

[0048] Hard carbon materials have suitable interlayer distances and abundant graphite microcrystalline domains, and are low in cost. They are widely used as the main negative electrode materials for sodium-ion batteries. Hard carbon is composed of microcrystals with a large number of defects and nanopores formed by stacking a few layers of small curved graphene sheets in a disordered manner. These defective carbon layers and nanopores can provide more active sites for the storage of sodium ions, and the size of the nanopores will affect the metallic properties of the sodium clusters formed in the pores.

[0049] Currently, element doping can expand the interlayer spacing of carbon materials, facilitating the insertion or extraction of sodium ions. At the same time, heteroatom doping can promote charge transfer and interaction between electrodes / electrolytes. Some external defects produced by doping can promote reaction activity and electronic conductivity, thereby improving the electrochemical performance of sodium-ion batteries.

[0050] One aspect of the present invention provides a method for preparing a hard carbon material, such as Figure 1 As shown, the method includes:

[0051] S11, providing plant biomass and a doping source containing a doping element.

[0052] The plant biomass may be aquatic plants, preferably emergent plants. The doping elements include one or more non-metallic elements.

[0053] S12, placing the plant biomass in a cultivation environment formed by the doping source for cultivation treatment.

[0054] The culture environment may include a hydroponic solution obtained by dissolving the doping source in deionized water.

[0055] Wherein, the doping source is used for cultivation treatment in the later growth stage of aquatic plants.

[0056] Among them, the cultivation treatment time is 5-10 days, the daily light duration is 6-10 hours; the temperature of the hydroponic solution is 18-23°C, and the room temperature of the cultivation environment is 23-27°C.

[0057] S13, using the cultivated plant biomass as a precursor raw material to prepare a hard carbon material containing doping elements.

[0058] In some embodiments, the doping element includes one or more of nitrogen, phosphorus, sulfur or boron.

[0059] As an example, the doping elements may include two non-metallic elements, and the doping source may be but is not limited to nitrogen-phosphorus co-doping, nitrogen-sulfur co-doping, nitrogen-boron co-doping, phosphorus-sulfur co-doping, phosphorus-boron co-doping or sulfur-boron co-doping.

[0060] As another example, the doping elements may include three non-metallic elements, and the doping source may be, but is not limited to, nitrogen-phosphorus-sulfur co-doping, nitrogen-phosphorus-boron co-doping, or phosphorus-sulfur-boron co-doping.

[0061] As another example, the doping elements may include four non-metallic elements, and the doping source may be nitrogen, phosphorus, sulfur and boron co-doping.

[0062] In some optional embodiments, the doping element includes nitrogen, and the doping source includes one or more of urea, thiourea, diammonium hydrogen phosphate, or ammonium pentaborate tetrahydrate.

[0063] In some optional embodiments, the doping element includes phosphorus, and the doping source includes one or more of diammonium hydrogen phosphate or ammonium dihydrogen phosphate.

[0064] In some optional embodiments, the doping element includes sulfur, and the doping source includes thiourea.

[0065] In some optional embodiments, the doping element includes boron, and the doping source includes ammonium pentaborate tetrahydrate.

[0066] In one embodiment, the doping elements include nitrogen, sulfur, phosphorus and boron, and the total molar concentration of nitrogen, sulfur, phosphorus and boron in the cultivation environment is (37.18-186) mg / L, and the mass concentration ratio of nitrogen, sulfur, phosphorus and boron is (15.8-79) mg / L: (10.55-52.75) mg / L: (5.86-29.3) mg / L: (4.97-24.8) mg / L. Furthermore, the total molar concentration of nitrogen, sulfur, phosphorus and boron in the cultivation environment is (74.36-148.72) mg / L, and the mass concentration ratios of nitrogen, sulfur, phosphorus and boron are (31.6-63.2) mg / L: (21.1-42.2) mg / L: (11.72-23.44) mg / L: (9.94-19.88) mg / L.

[0067] In one embodiment, the doping elements include nitrogen, sulfur and phosphorus, the total molar concentration of nitrogen, sulfur and phosphorus in the cultivation environment is (30.91-155) mg / L, and the mass concentration ratio of nitrogen, sulfur and phosphorus is (14.5-72.5) mg / L: (10.55-52.75) mg / L: (5.86-29.3) mg / L. Further, the total molar concentration of nitrogen, sulfur and phosphorus in the cultivation environment is (61.82-124) mg / L, and the mass concentration ratio of nitrogen, sulfur and phosphorus is (29-58) mg / L: (21.1-42.2) mg / L: (11.72-23.44) mg / L.

[0068] In one embodiment, the doping elements include nitrogen, sulfur and boron, the total molar concentration of nitrogen, sulfur and boron in the cultivation environment is (26.02-130) mg / L, and the mass concentration ratio of nitrogen, sulfur and boron is (10.5-52.5) ​​mg / L: (10.55-52.75) mg / L: (4.97-24.8) mg / L. Further, the total molar concentration of nitrogen, sulfur and boron in the cultivation environment is (52.04-104.08) mg / L, and the mass concentration ratio of nitrogen, sulfur and boron is (21-42) mg / L: (21.1-42.2) mg / L: (9.94-19.88) mg / L.

[0069] In one embodiment, the doping source includes thiourea, diammonium phosphate and ammonium pentaborate tetrahydrate; the mass concentration ratio of thiourea, diammonium phosphate and ammonium pentaborate tetrahydrate is (25-125) mg / L: (25-125) mg / L: (25-125) mg / L; correspondingly, the mass concentration ratio of nitrogen, sulfur, phosphorus and boron is (15.8-79) mg / L: (10.55-52.75) mg / L: (5.86-29.3) mg / L: (4.97-24.8) mg / L. Further, the mass concentration ratio of thiourea, diammonium hydrogen phosphate and ammonium pentaborate tetrahydrate is (50-100) mg / L: (50-100) mg / L: (50-100) mg / L, and correspondingly, the mass concentration ratio of nitrogen, sulfur, phosphorus and boron is (31.6-63.2) mg / L: (21.1-42.2) mg / L: (11.72-23.44) mg / L: (9.94-19.88) mg / L; preferably, the mass concentration ratio of thiourea, diammonium hydrogen phosphate and ammonium pentaborate tetrahydrate is 1:1:1. Thiourea, diammonium hydrogen phosphate and ammonium pentaborate tetrahydrate in a mass ratio of 1:1:1 are dissolved in deionized water to obtain a hydroponic solution.

[0070] In one embodiment, the doping source includes thiourea and diammonium hydrogen phosphate, and the mass concentration ratio of thiourea to diammonium hydrogen phosphate is (25-125) mg / L: (25-125) mg / L, and correspondingly, the mass concentration ratio of nitrogen, sulfur and phosphorus is (14.5-72.5) mg / L: (10.55-52.75) mg / L: (5.86-29.3) mg / L. Further, the mass concentration ratio of thiourea to diammonium hydrogen phosphate is (50-100) mg / L: (50-100) mg / L, and correspondingly, the mass concentration ratio of nitrogen, sulfur and phosphorus is (29-58) mg / L: (21.1-42.2) mg / L: (11.72-23.44) mg / L; preferably, the mass concentration ratio of thiourea to diammonium hydrogen phosphate is 1:1. Thiourea and diammonium hydrogen phosphate in a mass ratio of 1:1 were dissolved in deionized water to obtain a hydroponic solution.

[0071] In one embodiment, the doping source includes thiourea and ammonium pentaborate tetrahydrate, and the mass concentration ratio of thiourea to ammonium pentaborate tetrahydrate is (25-125) mg / L: (25-125) mg / L, and correspondingly, the mass concentration ratio of nitrogen, sulfur and boron is (10.5-52.5) ​​mg / L: (10.55-52.75) mg / L: (4.97-24.8) mg / L. Further, the mass concentration ratio of thiourea to ammonium pentaborate tetrahydrate is (50-100) mg / L: (50-100) mg / L, and correspondingly, the mass concentration ratio of nitrogen, sulfur and boron is (21-42) mg / L: (21.1-42.2) mg / L: (9.94-19.88) mg / L; preferably, the mass concentration ratio of thiourea to ammonium pentaborate tetrahydrate is 1:1. Thiourea and ammonium pentaborate tetrahydrate in a mass ratio of 1:1 were dissolved in deionized water to obtain a hydroponic solution.

[0072] In one embodiment, the steps of using cultivated plant biomass as a precursor raw material to prepare a hard carbon material containing doped elements include: washing and drying the precursor raw material and then crushing it to obtain a first precursor; using an alkaline solution to treat the first precursor to obtain a second precursor; subjecting the second precursor to a primary carbonization treatment to obtain a third precursor; subjecting the third precursor to a secondary carbonization treatment to obtain a hard carbon material containing doped elements, wherein the temperature of the primary carbonization treatment is lower than the temperature of the secondary carbonization treatment.

[0073] In some optional embodiments, the drying temperature of the precursor raw material is 60℃-120℃, including but not limited to 60℃, 70℃, 80℃, 90℃, 100℃, 110℃, 120℃, and the drying time of the precursor raw material is 6h-16h, including but not limited to 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h.

[0074] In some optional embodiments, the particle size of the first precursor is 1 μm-12 μm, including but not limited to 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, and 12 μm.

[0075] In some optional embodiments, the first precursor is subjected to alkaline treatment with an alkaline solution to obtain a second precursor, including: dispersing the first precursor in an alkaline solution to obtain a suspension, stirring at room temperature, washing with deionized water multiple times until the pH value of the suspension is neutral, and filtering and drying to obtain the second precursor.

[0076] In some optional embodiments, the volume ratio of the mass of the first precursor to the alkaline solution in the alkaline treatment is (15-30) g:300 ml, including but not limited to 15 g:300 ml, 20 g:300 ml, 25 g:300 ml, and 30 g:300 ml.

[0077] In some optional embodiments, the alkaline solution includes one or more of a potassium hydroxide solution or a sodium hydroxide solution.

[0078] In some optional embodiments, the mass fraction of the alkaline solution is 3%-6%, including but not limited to 3%, 4%, 5%, and 6%.

[0079] In some optional embodiments, the stirring time of the alkali treatment at room temperature is 6 h-12 h, including but not limited to 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, and 12 h.

[0080] In some optional embodiments, the temperature of the primary carbonization treatment is 500°C-800°C, including but not limited to 500°C, 600°C, 700°C, and 800°C.

[0081] In some optional embodiments, the time for a carbonization treatment is 1 h-6 h, including but not limited to 1 h, 2 h, 3 h, 4 h, 5 h, and 6 h.

[0082] In some optional embodiments, the temperature of the secondary carbonization treatment is 1000°C-1500°C, including but not limited to 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, and 1500°C.

[0083] In some optional embodiments, the time of the secondary carbonization treatment is 1 h-6 h, including but not limited to 1 h, 2 h, 3 h, 4 h, 5 h, and 6 h.

[0084] In one embodiment, the plant biomass is one or more of water hyacinth, hornwort, reed or Vallisneria.

[0085] The present application will be further described below with reference to specific embodiments and comparative examples.

[0086] Example 1

[0087] 375 mg of thiourea, 375 mg of diammonium hydrogen phosphate and 375 mg of ammonium pentaborate tetrahydrate were dissolved in 5000 ml of deionized water to obtain a hydroponic solution. Water hyacinths in the late growth period were placed in the hydroponic solution and cultivated for 7 days. During the cultivation process, the water temperature was maintained at 20°C, the room temperature was maintained at 25°C, and the light was maintained for 8 hours per day.

[0088] Among them, the types of doping elements in the cultivation environment are nitrogen, sulfur, phosphorus and boron, and the mass concentrations of nitrogen, sulfur, phosphorus and boron are 47.40 mg / L, 31.60 mg / L, 17.60 mg / L and 14.90 mg / L respectively.

[0089] The cultivated water hyacinth was used as a precursor raw material, washed with deionized water and dried at 80°C for 12 hours, and the dried product was crushed into water hyacinth powder with a particle size of 1 μm to obtain the first precursor. 20g of the first precursor was dispersed in 300ml of 5% sodium hydroxide solution by mass, stirred at room temperature for 8 hours, and a suspension was obtained after removing impurities. The suspension was placed in deionized water and stirred and dispersed, and then repeatedly washed with deionized water until pH = 7, and filtered and dried to obtain the second precursor.

[0090] Weigh 2 g of the second precursor and put it into a porcelain boat, and perform a carbonization treatment in a tubular furnace with nitrogen passing through, heating to 700°C at 5°C / min and keeping warm for 4 hours, then cool to 25°C to obtain the third precursor, and then perform a secondary carbonization treatment, heating to 1300°C at 5°C / min and keeping warm for 2 hours to obtain a hard carbon material containing doped elements N, S, P, and B.

[0091] Example 2

[0092] 250 mg of thiourea, 250 mg of diammonium hydrogen phosphate and 250 mg of ammonium pentaborate tetrahydrate were dissolved in 5000 ml of deionized water to obtain a hydroponic solution. Water hyacinths in the late growth period were placed in the hydroponic solution and cultivated for 7 days. During the cultivation process, the water temperature was maintained at 20°C, the room temperature was maintained at 25°C, and the light was maintained for 8 hours per day.

[0093] Among them, the types of doping elements in the cultivation environment are nitrogen, sulfur, phosphorus and boron, and the mass concentrations of nitrogen, sulfur, phosphorus and boron are 31.60 mg / L, 21.10 mg / L, 11.72 mg / L and 9.94 mg / L respectively.

[0094] The cultivated water hyacinth was used as a precursor raw material, washed with deionized water and dried at 120°C for 6 hours, and the dried product was crushed into water hyacinth powder with a particle size of 12 μm to obtain the first precursor. 30g of the first precursor was dispersed in 300ml of a 6% sodium hydroxide solution by mass, stirred at room temperature for 6 hours, and a suspension was obtained after removing impurities. The suspension was placed in deionized water and stirred and dispersed, and then repeatedly washed with deionized water until pH = 7, and filtered and dried to obtain the second precursor.

[0095] Weigh 2 g of the second precursor and put it into a porcelain boat, and perform a carbonization treatment in a tubular furnace with nitrogen passing through, heating to 700°C at 5°C / min and keeping warm for 4 hours, then cool to 25°C to obtain the third precursor, and then perform a secondary carbonization treatment, heating to 1300°C at 5°C / min and keeping warm for 2 hours to obtain a hard carbon material containing doped elements N, S, P, and B.

[0096] Example 3

[0097] 500 mg of thiourea, 500 mg of diammonium hydrogen phosphate and 500 mg of ammonium pentaborate tetrahydrate were dissolved in 5000 ml of deionized water to obtain a hydroponic solution. Water hyacinth in the late growth period was placed in the hydroponic solution and cultivated for 7 days. During the cultivation process, the water temperature was maintained at 20°C, the room temperature was maintained at 25°C, and the light was maintained for 8 hours per day.

[0098] Among them, the types of doping elements in the cultivation environment are nitrogen, sulfur, phosphorus and boron, and the mass concentrations of nitrogen, sulfur, phosphorus and boron are 63.20 mg / L, 42.20 mg / L, 23.44 mg / L and 19.88 mg / L respectively.

[0099] The cultivated water hyacinth was used as a precursor raw material, washed with deionized water and dried at 60°C for 16 hours, and the dried product was crushed into water hyacinth powder with a particle size of 6 μm to obtain the first precursor. 15g of the first precursor was dispersed in 300ml of a 3% sodium hydroxide solution by mass, stirred at room temperature for 12 hours, and a suspension was obtained after removing impurities. The suspension was placed in deionized water and stirred and dispersed, and then repeatedly washed with deionized water until pH = 7, and filtered and dried to obtain the second precursor.

[0100] Weigh 2 g of the second precursor and put it into a porcelain boat, and perform a carbonization treatment in a tubular furnace with nitrogen passing through, heating to 700°C at 5°C / min and keeping warm for 4 hours, then cool to 25°C to obtain the third precursor, and then perform a secondary carbonization treatment, heating to 1300°C at 5°C / min and keeping warm for 2 hours to obtain a hard carbon material containing doped elements N, S, P, and B.

[0101] Example 4

[0102] The preparation method of Example 4 is basically the same as the preparation method of Example 1, except that 125 mg of thiourea, 125 mg of diammonium hydrogen phosphate and 125 mg of ammonium pentaborate tetrahydrate are dissolved in 5000 ml of deionized water to obtain a hydroponic solution, that is, the masses of thiourea, diammonium hydrogen phosphate and ammonium pentaborate tetrahydrate are all 125 mg, and the rest are the same as in Example 1.

[0103] Among them, the types of doping elements in the cultivation environment are nitrogen, sulfur, phosphorus and boron, and the mass concentrations of nitrogen, sulfur, phosphorus and boron are 15.80 mg / L, 10.55 mg / L, 5.86 mg / L and 4.97 mg / L respectively.

[0104] Example 5

[0105] The preparation method of Example 5 is basically the same as the preparation method of Example 1, except that 625 mg of thiourea, 625 mg of diammonium hydrogen phosphate and 625 mg of ammonium pentaborate tetrahydrate are dissolved in 5000 ml of deionized water to obtain a hydroponic solution, that is, the masses of thiourea, diammonium hydrogen phosphate and ammonium pentaborate tetrahydrate are all 625 mg, and the rest are the same as in Example 1.

[0106] Among them, the types of doping elements in the cultivation environment are nitrogen, sulfur, phosphorus and boron, and the mass concentrations of nitrogen, sulfur, phosphorus and boron are 79.00 mg / L, 52.75 mg / L, 29.30 mg / L and 24.80 mg / L respectively.

[0107] Example 6

[0108] The preparation method of Example 6 is basically the same as the preparation method of Example 1, except that 375 mg of thiourea and 375 mg of diammonium hydrogen phosphate are dissolved in 5000 ml of deionized water to obtain a hydroponic solution, that is, ammonium pentaborate tetrahydrate is not added to the hydroponic solution, and the rest is the same as Example 1.

[0109] Among them, the types of doping elements in the cultivation environment are nitrogen, sulfur and phosphorus co-doped, and the mass concentrations of nitrogen, sulfur and phosphorus are 43.50 mg / L, 31.60 mg / L and 17.60 mg / L respectively.

[0110] Example 7

[0111] The preparation method of Example 7 is basically the same as the preparation method of Example 1, except that 375 mg of thiourea and 375 mg of ammonium pentaborate tetrahydrate are dissolved in 5000 ml of deionized water to obtain a hydroponic solution, that is, no diammonium hydrogen phosphate is added to the hydroponic solution, and the rest is the same as Example 1.

[0112] Among them, the types of doping elements in the cultivation environment are nitrogen, sulfur and boron co-doped, and the mass concentrations of nitrogen, sulfur and boron are 19.80 mg / L, 31.60 mg / L and 14.90 mg / L respectively.

[0113] Example 8

[0114] The preparation method of Example 8 is basically the same as the preparation method of Example 1, except that 375 mg of thiourea is dissolved in 5000 ml of deionized water to obtain a hydroponic solution, that is, diammonium hydrogen phosphate and ammonium pentaborate tetrahydrate are not added to the hydroponic solution, and the rest is the same as Example 1.

[0115] Among them, the types of doping elements in the cultivation environment are nitrogen and sulfur co-doped, and the mass concentrations of nitrogen and sulfur are 27.60 mg / L and 31.60 mg / L respectively.

[0116] Example 9

[0117] The preparation method of Example 9 is basically the same as the preparation method of Example 1, except that 375 mg of ammonium pentaborate tetrahydrate is dissolved in 5000 ml of deionized water to obtain a hydroponic solution, that is, thiourea and diammonium hydrogen phosphate are not added to the hydroponic solution, and the rest is the same as Example 1.

[0118] Among them, the types of doping elements in the cultivation environment are nitrogen and boron co-doped, and the mass concentrations of nitrogen and boron are 3.90 mg / L and 14.90 mg / L respectively.

[0119] Example 10

[0120] The preparation method of Example 10 is basically the same as the preparation method of Example 1, except that 375 mg of diammonium hydrogen phosphate is dissolved in 5000 ml of deionized water to obtain a hydroponic solution, that is, thiourea and ammonium pentaborate tetrahydrate are not added to the hydroponic solution, and the rest is the same as Example 1.

[0121] Among them, the types of doping elements in the cultivation environment are nitrogen and phosphorus co-doped, and the mass concentrations of nitrogen and phosphorus are 15.90 mg / L and 17.60 mg / L respectively.

[0122] Embodiment 11

[0123] The preparation method of Example 11 is basically the same as the preparation method of Example 1, except that during the first carbonization treatment, the temperature is raised to 500°C at 5°C / min and kept warm for 4 hours, that is, the temperature of the first carbonization treatment is 500°C, and the rest is the same as Example 1.

[0124] Example 12

[0125] The preparation method of Example 12 is basically the same as the preparation method of Example 1, except that: during the first carbonization treatment, the temperature is raised to 800°C at 5°C / min and kept warm for 6 hours, that is, the temperature of the first carbonization treatment is 800°C and the time is 6 hours, and the rest is the same as Example 1.

[0126] Example 13

[0127] The preparation method of Example 13 is basically the same as the preparation method of Example 1, except that during the secondary carbonization treatment, the temperature is raised to 1000°C at 5°C / min and kept warm for 2h, that is, the temperature of the secondary carbonization treatment is 1000°C, and the rest is the same as Example 1.

[0128] Embodiment 14

[0129] The preparation method of Example 14 is basically the same as the preparation method of Example 1, except that during the secondary carbonization treatment, the temperature is raised to 1500°C at 5°C / min and kept warm for 2h, that is, the temperature of the secondary carbonization treatment is 1500°C, and the rest is the same as Example 1.

[0130] Embodiment 15

[0131] The preparation method of Example 15 is basically the same as the preparation method of Example 1, except that the duckweed in the late growth stage is placed in a hydroponic solution for cultivation for 7 days, and the cultivated duckweed is used as the precursor raw material, that is, the plant biomass is replaced by the duckweed, and the rest is the same as Example 1.

[0132] Example 16

[0133] The preparation method of Example 16 is basically the same as the preparation method of Example 1, except that the reeds in the late growth period are placed in a hydroponic solution for cultivation for 7 days, and the cultivated reeds are used as precursor raw materials, that is, the plant biomass is replaced by the reeds, and the rest is the same as Example 1.

[0134] Comparative Example 1

[0135] The preparation method of Comparative Example 1 is substantially the same as that of Example 1, except that the hydroponic solution is replaced with deionized water, that is, the addition of the doping source is omitted, and the rest is the same as that of Example 1.

[0136] Comparative Example 2

[0137] The preparation method of Comparative Example 2 is basically the same as the preparation method of Example 1, except that: the water hyacinth is first cultivated with deionized water, and the second precursor is obtained after alkali treatment, and then the second precursor is soaked in a solution containing the doping element, that is, the water hyacinth is first cultivated and then doped with non-metallic elements, and the rest is the same as Example 1.

[0138] The water hyacinths in the late growth stage were placed in deionized water for 7 days. During the cultivation process, the water temperature was maintained at 20°C, the room temperature was maintained at 25°C, and the light was maintained for 8 hours per day.

[0139] The cultivated water hyacinth was used as a precursor raw material, washed with deionized water and dried at 80°C for 12 hours, and the dried product was crushed into water hyacinth powder with a particle size of 1 μm to obtain the first precursor. 20g of the first precursor was dispersed in 300ml of 5% sodium hydroxide solution by mass, stirred at room temperature for 8 hours, and a suspension was obtained after removing impurities. The suspension was placed in deionized water and stirred and dispersed, and then repeatedly washed with deionized water until pH = 7, and filtered and dried to obtain the second precursor.

[0140] 375 mg of thiourea, 375 mg of diammonium hydrogen phosphate and 375 mg of ammonium pentaborate tetrahydrate were dissolved in 5000 ml of deionized water to obtain a soaking solution, the second precursor was fully soaked in the soaking solution for 24 hours, and the fully soaked second precursor was dried to obtain a soaking precursor.

[0141] Weigh 2 g of the soaked precursor and put it into a porcelain boat, and perform a carbonization treatment in a tubular furnace with nitrogen passing through, heating to 700°C at 5°C / min and keeping warm for 4 hours, cool to 25°C to obtain a third precursor, and then perform a secondary carbonization treatment, heating to 1300°C at 5°C / min and keeping warm for 2 hours to obtain a hard carbon material containing doped elements N, S, P, and B.

[0142] Comparative Example 3

[0143] The preparation method of Comparative Example 3 is basically the same as the preparation method of Example 6, except that: the water hyacinth is first cultivated with deionized water, and the second precursor is obtained after alkali treatment, and then the second precursor is soaked in a solution containing the doping element, that is, the water hyacinth is first cultivated and then doped with non-metallic elements, and the rest is the same as Example 6.

[0144] The water hyacinths in the late growth stage were placed in deionized water for 7 days. During the cultivation process, the water temperature was maintained at 20°C, the room temperature was maintained at 25°C, and the light was maintained for 8 hours per day.

[0145] The cultivated water hyacinth was used as a precursor raw material, washed with deionized water and dried at 80°C for 12 hours, and the dried product was crushed into water hyacinth powder with a particle size of 1 μm to obtain the first precursor. 20g of the first precursor was dispersed in 300ml of 5% sodium hydroxide solution by mass, stirred at room temperature for 8 hours, and a suspension was obtained after removing impurities. The suspension was placed in deionized water and stirred and dispersed, and then repeatedly washed with deionized water until pH = 7, and filtered and dried to obtain the second precursor.

[0146] 375 mg of thiourea and 375 mg of diammonium hydrogen phosphate were dissolved in 5000 ml of deionized water to obtain a soaking solution, and the second precursor was fully soaked in the soaking solution for 24 hours. The fully soaked second precursor was dried to obtain a soaking precursor.

[0147] Weigh 2 g of the soaked precursor and put it into a porcelain boat, and perform a carbonization treatment in a tubular furnace with nitrogen passing through, heating to 700°C at 5°C / min and keeping warm for 4 hours, cool to 25°C to obtain a third precursor, and then perform a secondary carbonization treatment, heating to 1300°C at 5°C / min and keeping warm for 2 hours to obtain a hard carbon material containing doped elements N, S, and P.

[0148] Comparative Example 4

[0149] The preparation method of Comparative Example 4 is basically the same as the preparation method of Example 7, except that: the water hyacinth is first cultivated with deionized water, and the second precursor is obtained after alkali treatment, and then the second precursor is soaked in a solution containing the doping element, that is, the water hyacinth is first cultivated and then doped with non-metallic elements, and the rest is the same as Example 7.

[0150] The water hyacinths in the late growth stage were placed in deionized water for 7 days. During the cultivation process, the water temperature was maintained at 20°C, the room temperature was maintained at 25°C, and the light was maintained for 8 hours per day.

[0151] The cultivated water hyacinth was used as a precursor raw material, washed with deionized water and dried at 80°C for 12 hours, and the dried product was crushed into water hyacinth powder with a particle size of 1 μm to obtain the first precursor. 20g of the first precursor was dispersed in 300ml of 5% sodium hydroxide solution by mass, stirred at room temperature for 8 hours, and a suspension was obtained after removing impurities. The suspension was placed in deionized water and stirred and dispersed, and then repeatedly washed with deionized water until pH = 7, and filtered and dried to obtain the second precursor.

[0152] 375 mg of thiourea and 375 mg of ammonium pentaborate tetrahydrate are dissolved in 5000 ml of deionized water to obtain a soaking solution, the second precursor is fully soaked in the soaking solution for 24 hours, and the fully soaked second precursor is dried to obtain a soaking precursor.

[0153] Weigh 2 g of the soaked precursor and put it into a porcelain boat, and perform a carbonization treatment in a tubular furnace with nitrogen passing through, heating to 700°C at 5°C / min and keeping warm for 4 hours, cool to 25°C to obtain a third precursor, and then perform a secondary carbonization treatment, heating to 1300°C at 5°C / min and keeping warm for 2 hours to obtain a hard carbon material containing doped elements N, S, and B.

[0154] The raw materials and related parameters in the preparation methods of Examples 1 to 16 and Comparative Examples 1 to 4 are shown in Table 1 below, where “-” means untreated.

[0155] Table 1

[0156]

[0157]

[0158] Preparation of sodium ion batteries:

[0159] The electrode preparation process of the negative electrode material mainly includes mixing, coating, drying, cutting and weighing. The specific preparation process is as follows. Mixing: The prepared active material (i.e., the hard carbon material prepared in the embodiment and the comparative example) is mixed with the conductive agent (Super P) and the binder (CMC+SBR, the mass ratio of CMC and SBR is 4:6) in a mass ratio of 8:1:1, and the slurry is prepared with deionized water as the solvent. Stir in a magnetic stirrer for 24 hours to make the slurry mix evenly. Coating: Pre-laminate the copper foil on a flat and smooth glass plate, and then pour the mixed slurry on the copper foil, and use a coater to coat the slurry on the copper foil, try to spread the slurry evenly and flatly, with a thickness of 150um. Drying: Place the copper foil coated with the slurry in a vacuum oven and dry it at 80°C for 12 hours. Weighing of cut pieces: Take out the dried electrode pieces and use a manual punching and cutting machine to cut the electrode pieces into discs with a diameter of 14 mm. Then weigh the mass of each electrode piece on an electronic balance and calculate the mass of the active substance.

[0160] The battery assembly process is carried out in a glove box filled with argon. The assembled battery model is a CR2032 button battery. A metal sodium sheet (diameter 15.6mm) is used as the counter electrode of the half-cell, Whatman glass fiber (diameter 18mm) is used as the diaphragm, the electrolyte is 1mol / L NaClO4, the solvent in the electrolyte is ethylene carbonate (EC) and dimethyl carbonate (DEC) in a volume ratio of 1:1, and contains 5% fluoroethylene carbonate (FEC). The battery assembly process is: place the battery electrode in the center of the positive electrode shell, then add 40pL of electrolyte, put in the glass fiber diaphragm and add 40pL of electrolyte again, then place the metal sodium sheet on the diaphragm, and finally add the gasket, shrapnel, and negative electrode shell in turn. Finally, the battery assembly is completed after the sealing machine is encapsulated. After the battery is assembled, it needs to be left to stand for more than 8 hours. After standing, the battery clip can be placed on the charge and discharge instrument for electrochemical performance testing.

[0161] Test Case

[0162] The mass percentage of each doping element in the second precursor prepared by the above embodiment and the immersion precursor prepared by the comparative example, as well as the mass percentage of each doping element in the hard carbon material were tested by combining a scanning electron microscope (SEM) and an energy dispersive spectrometer (EDS). The test results are shown in Table 2, where “ / ” means not detected.

[0163] The sodium ion battery obtained by using the hard carbon material prepared by the above embodiment and comparative example was tested for the first charge specific capacity, the first discharge specific capacity and the first coulomb efficiency. The test results are shown in Table 2. Among them, the charge and discharge capacity test and the first coulomb efficiency test used the charge and discharge instrument of Blue Electric Company, the test temperature was constant at 25°C, the battery charge and discharge voltage range was set to 0-3V, and the constant current density was 50mA / g for charge and discharge. After each charge and discharge, let it stand for 3 minutes before the next charge and discharge.

[0164] Table 2

[0165]

[0166] It can be seen from Tables 1 and 2 that the first charge specific capacity, first discharge specific capacity and first coulombic efficiency of Example 1 are significantly higher than those of Comparative Example 2, the first charge specific capacity, first discharge specific capacity and first coulombic efficiency of Example 6 are significantly higher than those of Comparative Example 3, and the first charge specific capacity, first discharge specific capacity and first coulombic efficiency of Example 7 are significantly higher than those of Comparative Example 4, indicating that compared with conventional biomass material crushing, alkali treatment and then element doping, the present application performs element doping in the cultivation environment of cultivation treatment, which can significantly improve the electrochemical properties of hard carbon materials.

[0167] It can be seen from Examples 1 to 5 that when the total molar concentration of each doping element and the mass concentration ratio of each doping element in the cultivation environment are within an appropriate range, the sodium ion battery prepared from the corresponding hard carbon material can simultaneously have good first charge specific capacity, first discharge specific capacity and first coulombic efficiency.

[0168] It can be seen from Examples 1 to 10 and Comparative Examples 2 to 4 that, due to the synergistic effect of multiple heteroatoms, co-doping with more types of elements can produce more defects and active sites, increase the interlayer spacing of the hard carbon material, and further optimize the electron distribution around the carbon atoms, thereby improving the conductivity of the material.

[0169] It can be seen from Example 1 and Example 11-Example 14 that when the temperature and time of the primary carbonization, as well as the temperature and time of the secondary carbonization are all within an appropriate range, the sodium ion battery prepared from the corresponding hard carbon material can simultaneously have good first charge specific capacity, first discharge specific capacity and first coulombic efficiency.

[0170] It can be seen from Example 1, Example 15 and Example 16 that the preparation method of the hard carbon material provided in the present application is applicable to a variety of emergent plants. Furthermore, among different emergent plants, the hard carbon material prepared from Eichhornia crassipes has the highest total content of doped elements, and the prepared sodium ion battery also has better first charge specific capacity, first discharge specific capacity and first coulombic efficiency.

[0171] It can be found from the above-mentioned Examples 1 to 16 and Comparative Examples 1 to 4 that the present application adsorbs the doping elements in the doping source into the plant biomass through the bioaccumulation of the plant biomass during the cultivation process, thereby realizing the in situ combination of the doping elements and the plant biomass material, so that the prepared hard carbon material can provide more active sites for adsorbing sodium ions, thereby improving the sodium storage performance of the hard carbon material and significantly improving the electrochemical performance of the prepared sodium ion battery.

[0172] Furthermore, the present application uses bio-enrichment of plant biomass during the cultivation process, and the preparation process is simple, and it is very easy to achieve free combination and co-doping of multiple elements, which is conducive to improving the surface and functional group functionalization of hard carbon negative electrode materials, introducing more reversible defects and sodium ion reaction active sites, and improving the specific capacity and rate performance of hard carbon negative electrode materials. In addition, the preparation steps are simple, and the raw materials are cheap and easy to obtain, which is conducive to large-scale production.

[0173] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0174] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a hard carbon material, characterized in that: The preparation method comprises: Providing plant biomass and a doping source containing a doping element, wherein the doping element includes a non-metallic element; placing the plant biomass in a cultivation environment formed by the doping source for cultivation treatment; The cultivated plant biomass is used as a precursor raw material to prepare a hard carbon material containing doping elements.

2. The preparation method according to claim 1, characterized in that: The non-metallic elements include one or more of nitrogen, phosphorus, sulfur or boron.

3. The preparation method according to claim 2, characterized in that: The method satisfies at least one of the following conditions: (1) The doping element includes nitrogen, and the doping source includes one or more of urea, thiourea, diammonium hydrogen phosphate or ammonium pentaborate tetrahydrate; (2) the doping element includes phosphorus, and the doping source includes one or more of diammonium hydrogen phosphate or ammonium dihydrogen phosphate; (3) The doping element includes sulfur, and the doping source includes thiourea; (4) The doping element includes boron, and the doping source includes ammonium pentaborate tetrahydrate.

4. The preparation method according to claim 2, characterized in that: The cultivation process satisfies at least one of the following conditions: (1) The total mass concentration of the nitrogen element, the sulfur element, the phosphorus element and the boron element in the cultivation environment is (37.18-186) mg / L, and the mass concentration ratio of the nitrogen element, the sulfur element, the phosphorus element and the boron element is (15.8-79) mg / L: (10.55-52.75) mg / L: (5.86-29.3) mg / L: (4.97-24.8) mg / L; (2) The total mass concentration of the nitrogen element, the sulfur element and the phosphorus element in the cultivation environment is (30.91-155) mg / L, and the mass concentration ratio of the nitrogen element, the sulfur element and the phosphorus element is (14.5-72.5) mg / L: (10.55-52.75) mg / L: (5.86-29.3) mg / L; (3) The total mass concentration of the nitrogen element, the sulfur element and the boron element in the cultivation environment is (26.02-130) mg / L, and the mass concentration ratio of the nitrogen element, the sulfur element and the boron element is (10.5-52.5) ​​mg / L: (10.55-52.75) mg / L: (4.97-24.8) mg / L.

5. The preparation method according to claim 3, characterized in that: The cultivation process satisfies at least one of the following conditions: (1) The doping source comprises thiourea, diammonium hydrogen phosphate and ammonium pentaborate tetrahydrate; the mass concentration ratio of the thiourea, the diammonium hydrogen phosphate and the ammonium pentaborate tetrahydrate is (25-125) mg / L: (25-125) mg / L: (25-125) mg / L; (2) The doping source comprises thiourea and diammonium phosphate; the mass concentration ratio of the thiourea to the diammonium phosphate is (25-125) mg / L: (25-125) mg / L; (3) The doping source comprises thiourea and ammonium pentaborate tetrahydrate; the mass concentration ratio of the thiourea to the ammonium pentaborate tetrahydrate is (25-125) mg / L: (25-125) mg / L.

6. The preparation method according to claim 1, characterized in that: The step of using the cultivated plant biomass as a precursor raw material to prepare a hard carbon material containing doping elements comprises: The precursor raw material is washed and dried and then crushed to obtain a first precursor; Using an alkaline solution to perform alkaline treatment on the first precursor to obtain a second precursor; Carrying out a carbonization treatment on the second precursor to obtain a third precursor; The third precursor is subjected to a secondary carbonization treatment to obtain the hard carbon material containing the doping element, wherein the temperature of the primary carbonization treatment is lower than the temperature of the secondary carbonization treatment.

7. The preparation method according to claim 6, characterized in that: The step of obtaining the hard carbon material containing the doping element satisfies at least one of the following conditions: (1) The particle size of the first precursor is 1 μm-12 μm; (2) treating the first precursor with an alkaline solution to obtain the second precursor comprises dispersing the first precursor in an alkaline solution to obtain a suspension, stirring at room temperature, washing with deionized water for multiple times until the pH value of the suspension is neutral, and filtering and drying to obtain the second precursor; (3) The temperature of the primary carbonization treatment is 500° C.-800° C.; (4) The time of the primary carbonization treatment is 1h-6h; (5) The temperature of the secondary carbonization treatment is 1000° C.-1500° C.; (6) The time of the secondary carbonization treatment is 1h-6h.

8. The preparation method according to claim 1, characterized in that: The plant biomass comprises one or more of water hyacinth, hornwort, reed or Vallisneria.

9. A hard carbon material, characterized in that: The method is prepared according to any one of claims 1 to 8.

10. A sodium ion battery, characterized in that: The hard carbon material comprises the hard carbon material prepared by the preparation method according to any one of claims 1 to 8 or the hard carbon material according to claim 9.

Citation Information

Patent Citations

  • Preparation method of self-absorption nitrogen-sulfur doped porous carbon

    CN108373154A

  • A preparation method of porous nitrogen-doped carbon material based on fungal biomass and application thereof

    CN108987122A

  • Nitrogen and phosphorus-doped biomass-based carbon quantum dots, application and method for cell imaging detection by using the same

    CN110791289A

  • Microalgal bio-based nitrogen-doped carbon material as well as preparation method and application thereof

    CN111943162A

  • Biomass hard carbon negative electrode material and preparation method and application thereof