Preparation method of long-afterglow luminescent carbon dot material taking waste plastic as raw material

By solubilizing waste plastic with auxiliary reactants such as glycol and urea, combined with reduced pressure and heat treatment, long afterglow luminescent carbon dot material is prepared, which solves the problem of waste plastic treatment and reuse, and achieves high The production of value-added materials is suitable for lighting, imaging and other fields.

CN118929638APending Publication Date: 2024-11-12CHONGQING UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411160400.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art cannot effectively treat and reuse waste plastics, resulting in environmental pollution and waste of resources, and landfill and incineration methods cause pollution to the environment.

Method used

The waste plastic is mixed with auxiliary reactants such as ethylene glycol and urea by using solvent-thermal method or microwave method, and the volatile substances are removed after decompression or direct heating. Then, ultrasonic, centrifugation, dialysis and freeze-drying are performed to prepare long afterglow luminescent carbon dots. Material.

Benefits of technology

It realizes the degradation and reprocessing of waste plastics, prepares carbon dot materials with excellent long afterglow luminescence performance, solves the problems of plastic pollution and resource regeneration, and converts low-value-added waste plastics into high-value-added long afterglow luminescence. Materials, suitable for a variety of application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929638A_ABST
    Figure CN118929638A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a long afterglow luminescent carbon dot material using waste plastics as a raw material, and relates to the field of material preparation, and the preparation method comprises the following steps: S1, mixing the waste plastics, a reactant and an auxiliary reactant, and converting a mixture system into a homogeneous phase by using a solvothermal method or a microwave method; the reactant is ethylene glycol; the auxiliary reactant is urea or a derivative thereof; s2, after the reaction is completed, volatile substances are removed through a pressure reduction method or a direct heating method, and a solid crude product is obtained; and S3, dissolving the solid crude product in deionized water, and sequentially carrying out ultrasonic treatment, centrifugation, dialysis and freeze drying treatment to obtain the long-afterglow luminescent carbon dot material. According to the method, the waste plastic is used as the raw material, the waste plastic is firstly degraded into small molecules through the provided method, the small molecules are synthesized into the carbon dot material with long afterglow luminescence performance in the presence of the catalyst under the specific reaction pressure intensity and the reaction temperature, upgrading and recycling of the waste plastic can be effectively achieved, and the problems of plastic pollution and resource regeneration are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material preparation, and in particular to a method for preparing a long afterglow luminescent carbon dot material using waste plastics as raw materials. Background Art

[0002] Polymer materials are widely used, bringing great convenience to daily life and industrial development. However, the generation of waste plastics is also a major problem that cannot be ignored at the social level. At present, the global methods for dealing with waste plastics include landfill, incineration, recycled granulation and pyrolysis. Among them, landfill and incineration will cause pollution to the environment. If plastic products remain in farmland for a long time, it will affect the absorption of water and nutrients by crops, inhibit the growth and development of crops, and cause a reduction in crop yields. If animals eat plastic products by mistake, they will suffer from indigestion or even death. This not only puts great pressure on the environment, but also fails to achieve effective reuse of resources. Upcycling of waste plastics is a very challenging problem. If the degradation and reprocessing of waste plastics can be achieved in one step, resources can be effectively reused. Summary of the invention

[0003] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing a long afterglow luminescent carbon dot material using waste plastics as raw materials, thereby solving the major environmental pollution problem of "white pollution" of existing waste plastics, and realizing the recycling of waste resources, and preparing a carbon dot material with excellent long afterglow luminescent performance.

[0004] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:

[0005] Provided is a method for preparing a long afterglow luminescent carbon dot material using waste plastic as raw material, comprising the following steps:

[0006] S1: After mixing waste plastics, a reactant and an auxiliary reactant, the mixture system is transformed into a homogeneous phase using a solvent thermal method or a microwave method; the reactant is ethylene glycol; the auxiliary reactant is urea or its derivatives;

[0007] S2: After the reaction is completed, the volatile substances are removed by decompression or direct heating to obtain a solid crude product;

[0008] S3: After dissolving the solid crude product in deionized water, the solid crude product is sequentially subjected to ultrasonic treatment, centrifugation, dialysis and freeze-drying treatment to obtain a long afterglow luminescent carbon dot material.

[0009] Furthermore, when the mixture system is converted into a homogeneous phase using a solvothermal method, the reaction temperature of the solvothermal reaction is 200-300° C., and the reaction time is 6 h to 12 h.

[0010] Furthermore, when the mixture system is converted into a homogeneous phase using a microwave method, the microwave reaction power is 500-700 W and the reaction time is 50-200 s.

[0011] Furthermore, when the volatile substances are removed by the reduced pressure method in step S2, the reaction pressure is set to 1010-1010000 Pa and the reaction temperature is set to 60-200°C.

[0012] Furthermore, when the volatile substances are removed by direct heating in step S2, the reaction temperature is set to 200-300°C.

[0013] Furthermore, during dialysis, the molecular weight cut-off is 100-500.

[0014] Furthermore, the waste plastics are a combination of one or more of discarded polyolefin materials, aliphatic polyester materials, aromatic polyester materials, polycarbonate, polyurethane, nylon or unsaturated polyester.

[0015] Furthermore, the auxiliary reaction agent is urea, 1,1-dimethylurea, 1,3-dimethylurea, tetramethylurea, thiourea, 2-pyrrolidone, tetrahydro-2-pyrimidinone, ethyl carbamate, uric acid, urea phosphate or urea.

[0016] Furthermore, the mass ratio of waste plastics, reactants and auxiliary reactants is 1:5-50:0.2-10.

[0017] The beneficial effects of the present invention are:

[0018] The present invention uses waste plastics as raw materials, and uses the provided method to first degrade the waste plastics into small molecules, and the small molecules synthesize carbon dot materials with long afterglow luminescence performance in the presence of a catalyst and a specific reaction pressure and reaction temperature, thereby realizing the "top-down" and "bottom-up" transformations in sequence, which can effectively realize the upgrading and recycling of waste plastics and solve the problems of plastic pollution and resource regeneration. The long afterglow luminescent carbon dot materials prepared from waste plastics as raw materials can prepare low-value-added waste plastics into high-value-added long afterglow luminescent materials, which can be applied to many fields such as lighting, imaging, road signs and warnings, commodity anti-counterfeiting, information encryption, biological identification, and sensing. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the appearance of the long afterglow luminescent carbon dot material prepared in Example 1;

[0020] Figure 2 This is an infrared spectrum of the afterglow carbon dot material prepared by the present invention;

[0021] Figure 3 This is a phosphorescence spectrum of the long afterglow luminescent carbon dot material prepared in Example 1;

[0022] Figure 4 This is a phosphorescence spectrum of the long afterglow luminescent carbon dot material prepared in Example 2;

[0023] Figure 5 This is a phosphorescence spectrum of the long afterglow luminescent carbon dot material prepared in Example 3;

[0024] Figure 6 This is the phosphorescence spectrum of the long afterglow luminescent carbon dot material prepared in Example 4. DETAILED DESCRIPTION

[0025] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0026] The waste plastics used in the embodiments of the present invention are household waste plastics and experimental waste plastics collected within the scope of Chongqing University of Technology, including waste bottle pieces, packing tapes, food packaging, medicine packaging, sample bags, disposable plastic experimental consumables, etc. In specific implementation, waste polyolefin materials, aliphatic polyester materials, aromatic polyester materials, polycarbonate, polyurethane, nylon, unsaturated polyester or other plastic products can be used in combination of one or more.

[0027] Cut the waste plastic into pieces. The purpose of cutting into pieces is to control the weight component, facilitate laboratory experiments, and facilitate placement into the reactor. In specific implementation, in large-scale preparation, if the reactor feed port is larger than the waste plastic, no cutting is required.

[0028] Example 1

[0029] Take 2g of waste plastic fragments, 20mL of ethylene glycol and 2g of urea and put them in a reactor, and react the reactor at 275℃ for 6h. After the reaction is completed, use the decompression method, set the reaction pressure to 3.33kPa, react at 125℃ for 1h, remove all volatile substances, add 50mL of deionized water to dissolve the obtained crude product, use a centrifuge at a speed of 4000r / min, centrifuge for 1h, remove the supernatant, pour the residue into a dialysis bag with a molecular weight cutoff of 200. In specific implementation, a dialysis bag with a molecular weight cutoff of 100, 300 or 500 can also be used; put it into a beaker filled with 300ml of deionized water for dialysis, and the dialysis time is 48h. After the dialysis is completed, take the supernatant in the dialysis bag and use a freeze dryer model FDS-2000 for freeze drying. The internal pressure is 0pa, the temperature is -80℃, and the freeze drying time is 72h to obtain the following Figure 1 The long afterglow luminescent carbon dot material shown in the figure, in which the red area is the matrix and the inner yellow area is the carbon dot. Figure 1 It can be seen that the prepared long afterglow luminescent carbon dot material is in a quasi-spherical shape, with a diameter of less than 10 nm, and is dispersed between the matrix.

[0030] In specific implementation, the reaction pressure of the reduced pressure method can also be 1.01, 2, 4, 5, 10, 100, 300, 500, 700 or 1010 kPa, any one within the range of 1010 to 1010000 Pa; the reaction temperature can also be 60, 100, 150 or 200°C, any one within the range of 60-200°C.

[0031] Example 2

[0032] 2 g of waste plastic fragments, 20 mL of ethylene glycol and 2 g of 1,1-dimethylurea were placed in a reactor, and the reactor was reacted at 275 ° C for 6 h. After the reaction was completed, the reaction pressure was set to 3.33 kPa using a decompression method, and the reaction was carried out at 125 ° C for 1 h. After removing all volatile substances, 50 mL of deionized water was added to dissolve the obtained crude product, and the same ultrasonic, centrifugal, dialysis and freeze-drying treatment as in Example 1 was used to obtain a long afterglow luminescent carbon dot material.

[0033] Example 3

[0034] 2 g of waste plastic fragments, 20 mL of ethylene glycol and 2 g of 1,3-dimethylurea were placed in a reactor, and the reactor was reacted at 275 ° C for 6 hours. After the reaction was completed, the reaction pressure was set to 3.33 kPa using a decompression method, and the reaction was carried out at 125 ° C for 1 hour. After removing all volatile substances, 50 mL of deionized water was added to dissolve the obtained crude product, and the same ultrasonic, centrifugal, dialysis and freeze-drying treatment as in Example 1 was used to obtain a long afterglow luminescent carbon dot material.

[0035] Example 4

[0036] 2 g of waste plastic fragments, 20 mL of ethylene glycol and 2 g of tetramethylurea were placed in a reactor, and the reactor was reacted at 275 ° C for 6 h. After the reaction was completed, the reaction pressure was set to 3.33 kPa using a decompression method, and the reaction was carried out at 125 ° C for 1 h. After removing all volatile substances, 50 mL of deionized water was added to dissolve the obtained crude product, and the same ultrasonic, centrifugal, dialysis and freeze-drying treatment as in Example 1 was used to obtain a long afterglow luminescent carbon dot material.

[0037] In other embodiments of the present invention, the mass ratio of waste plastics, ethylene glycol and auxiliary reactant can also be 1:5:0.2, 1:30:5, 1:45:8 or 1:50:10, any ratio within the range of 1:5-50:0.2-10.

[0038] In other embodiments of the present invention, the auxiliary reaction agent can also be any one of 1,1-dimethylurea, 1,3-dimethylurea, tetramethylurea, thiourea, 2-pyrrolidone, tetrahydro-2-pyrimidone, ethyl carbamate, uric acid, urea phosphate or urea.

[0039] When the mixture system is converted into a homogeneous phase by a solvothermal method, the reaction temperature can also be 200, 225, 250 or 300° C., any one of which can be selected in the range of 200-300° C. The reaction time can also be 8, 10 or 12 hours, any one of which can be selected in the range of 6-12 hours.

[0040] The mixture system can also be transformed into a homogeneous phase by microwave method or other methods that do not change the properties of the mixture. When the microwave method is used, the microwave reaction power is 500, 550, 600, 650 or 700 W, any one of which can be selected within the range of 500-700 W; and the reaction time is 50, 100, 150 or 200 s, any one of which can be selected within the range of 50-200 s.

[0041] When removing all volatile substances from the reaction product, direct heating method or other methods that do not change the properties of the mixture can also be used. When using the direct heating method, the specific operation is to place the homogeneous mixture obtained by the reaction in a reactor, directly heat the reactor to 200-300°C, and keep ventilation during the heating process to allow the volatile substances to escape from the reactor.

[0042] Example 5

[0043] The long afterglow luminescent carbon dot materials prepared in Examples 1-4 were subjected to infrared spectrum detection respectively. The detection results are as follows: Figure 2 As shown by Figure 2 It can be seen that in the infrared spectra of the long afterglow luminescent carbon dot materials prepared in Examples 1-4, at 1750cm -1 There is a characteristic peak of carbonyl (C=O) stretching vibration at 1150cm -1 There is a characteristic peak of CO stretching vibration at 3300cm -1 There is a characteristic peak caused by the stretching vibration of the NH group of the amino group, which proves that the structure of this material contains amino functional groups. -1 There are sp 2 The C=C stretching vibration of the structure is a characteristic peak of graphite, which proves that the material structure has a graphite core structure. That is, the method provided by the present invention can prepare quasi-spherical long afterglow luminescent carbon dot materials.

[0044] The long afterglow luminescent carbon dot materials obtained in Examples 1-4 were respectively subjected to phosphorescence spectrum detection, and the detection results are as follows: Figure 3-6 As shown, Figure 3-6 The phosphorescence spectra of the long afterglow luminescent carbon dot materials obtained in Examples 1-4 are shown in FIG. Figure 3-6 It can be seen that the method of the present invention can be used to prepare a long afterglow luminescent carbon dot material which emits green light with a wavelength between 500-550 nm under the excitation of a light source with a wavelength of 365 nm.

Claims

1. A method for preparing a long afterglow luminescent carbon dot material using waste plastics as raw materials, It is characterized in that The steps include: S1: After mixing waste plastics, a reactant and an auxiliary reactant, the mixture system is transformed into a homogeneous phase using a solvent thermal method or a microwave method; the reactant is ethylene glycol; the auxiliary reactant is urea or its derivatives; S2: After the reaction is completed, volatile substances are removed by decompression or direct heating to obtain a solid crude product; S3: After dissolving the solid crude product in deionized water, the solid crude product is sequentially subjected to ultrasonic treatment, centrifugation, dialysis and freeze-drying treatment to obtain a long afterglow luminescent carbon dot material.

2. The method for preparing the long afterglow luminescent carbon dot material using waste plastic as raw material according to claim 1, It is characterized in that When the mixture system is converted into a homogeneous phase using a solvothermal method, the reaction temperature of the solvothermal reaction is 200-300° C., and the reaction time is 6 h to 12 h.

3. The method for preparing the long afterglow luminescent carbon dot material using waste plastic as raw material according to claim 1, It is characterized in that When the mixture system is converted into a homogeneous phase using a microwave method, the microwave reaction power is 500-700 W and the reaction time is 50-200 s.

4. The method for preparing the long afterglow luminescent carbon dot material using waste plastic as raw material according to claim 1, It is characterized in that When the step S2 uses a reduced pressure method to remove volatile substances, the reaction pressure is set to 1010-1010000 Pa and the reaction temperature is set to 60-200°C.

5. The method for preparing the long afterglow luminescent carbon dot material using waste plastic as raw material according to claim 1, It is characterized in that When the step S2 uses a direct heating method to remove volatile substances, the reaction temperature is set at 200-300°C.

6. The method for preparing the long afterglow luminescent carbon dot material using waste plastic as raw material according to claim 1, It is characterized in that During the dialysis, the molecular weight cut-off is 100-500.

7. The method for preparing the long afterglow luminescent carbon dot material using waste plastic as raw material according to claim 1, It is characterized in that The waste plastics are a combination of one or more of discarded polyolefin materials, aliphatic polyester materials, aromatic polyester materials, polycarbonate, polyurethane, nylon or unsaturated polyester.

8. The method for preparing the long afterglow luminescent carbon dot material using waste plastic as raw material according to claim 1, It is characterized in that The auxiliary reaction agent is urea, 1,1-dimethylurea, 1,3-dimethylurea, tetramethylurea, thiourea, 2-pyrrolidone, tetrahydro-2-pyrimidone, ethyl carbamate, uric acid, urea phosphate or urea.

9. The method for preparing the long afterglow luminescent carbon dot material using waste plastic as raw material according to claim 1, It is characterized in that The mass ratio of the waste plastic, the reactant and the auxiliary reactant is 1:5-50:0.2-10.

Citation Information

Cited By

  • Polymer with thermally enhanced long afterglow characteristic as well as preparation method and application thereof

    CN120329693A