Preparation method of waste rubber magnetic separation and recovery and rubber-derived porous carbon electrode material
By separating magnetic powder from rubber magnets through liquid nitrogen freezing and high-speed shearing, and combining it with a carbonization-activation process, a porous carbon electrode material suitable for supercapacitors was prepared. This solved the problem of recycling and reusing waste rubber magnets, achieving efficient resource utilization and environmental protection.
Patent Information
- Application Number
- CN202411124533.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
AI Technical Summary
The recycling and reuse of waste rubber magnets cannot maximize resource utilization, and rubber cannot be directly used for reprocessing after the rubber magnets are scrapped, resulting in resource waste and environmental pollution.
Rubber and magnetic powder were separated by liquid nitrogen freezing combined with high-speed shearing. The magnetic powder was recovered by calcination, and the rubber was carbonized and activated to prepare porous carbon for use as electrode material for supercapacitors. Hydroxide was used as an activator, and a mixed conductive agent was coated on nickel foam for electrochemical testing.
The effective separation of rubber magnets and the secondary utilization of resources were achieved. The prepared porous carbon electrode material exhibited good electrochemical performance and was suitable for supercapacitors.
Smart Images

Figure CN118929662A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of magnetic recovery of waste rubber and preparation of capacitive porous carbon, and in particular to separation of magnetic rubber and magnetic powder from waste rubber and preparation of porous carbon electrode by rubber carbon / activation. Background Art
[0002] Rubber magnets are soft, elastic and twistable magnets made of bonded ferrite powder and synthetic rubber through extrusion, calendering, injection and other molding processes. They are widely used in micro motors, home appliances, automobiles, etc. However, if rubber magnets are not properly disposed of after being scrapped during normal use and cascade utilization, it will lead to huge waste of resources and serious environmental pollution. The recycling and reuse of waste rubber magnets is the key to maximizing the value of resources.
[0003] Since the bonding between magnetic powder and rubber depends on coupling agent during the preparation of rubber magnets, mechanical means can be used to effectively strip ferrite from the rubber magnet matrix, and it can be reused after calcination to remove the surface coupling agent; while rubber has undergone high-temperature cross-linking and cannot be directly used for the re-preparation of rubber magnets. Rubber is rich in carbon atoms and is a precursor for preparing porous carbon materials, so the carbonization-activation method can be used to prepare rubber-based electrode materials for supercapacitors. Summary of the invention
[0004] The purpose of the present invention is to provide a method for magnetic separation and recovery of waste rubber and preparation of rubber-derived porous carbon electrode materials in view of the deficiencies of the prior art, which is characterized by comprising the following steps:
[0005] A method for magnetic separation and recovery of waste rubber and preparation of rubber-derived porous carbon electrode materials, characterized by comprising the following steps:
[0006] (1) Separation of rubber and magnetic powder in rubber magnets: 10 g of waste rubber magnets were placed in a liquid nitrogen tank for 5 min, then transferred to a high-speed crusher for 30 min, and the detached ferrite magnetic powder was separated by adsorption using a magnet. The operation was repeated several times until no obvious magnetic powder particles were adsorbed. The magnetic powder particles were calcined in air and reused.
[0007] (2) The separated rubber particles are pre-carbonized at 250-350°C for 1 h to remove the volatile components on the surface, and then mixed with an activator in a mass ratio of 1:1-1:4 and placed in a nickel crucible. A proper amount of alcohol is added and stirred to dry. Finally, the particles are placed in a horizontal tube furnace and treated at 600-900°C for 0.5-2 h under an inert atmosphere. After cooling to room temperature, they are washed with dilute hydrochloric acid and deionized water until neutral.
[0008] (3) The porous carbon, PVDF binder and conductive agent obtained in step 2 were mixed in a mass ratio of 8:1:1, and a small amount of N-methylpyrrolidone was added to grind into a paste, and then evenly coated on 1×1 cm2 nickel foam, placed in an oven at 80 ºC to dry the pressed sheet for subsequent testing;
[0009] (4) During the test, Hg / HgO and Pt sheets were used as reference electrodes and counter electrodes, porous carbon@nickel foam was used as working electrode, and 6 M potassium hydroxide aqueous solution was used as electrolyte. The electrochemical tests mainly included cyclic voltammetry (CV), constant current charge and discharge (GCD) and electrochemical impedance spectroscopy.
[0010] The activator comprises potassium hydroxide and sodium hydroxide, the conductive agent is conductive carbon black or acetylene black, and the porous carbon loading on the nickel foam is 2-5 mg / cm2.
[0011] The voltage window of the electrochemical test is -1 to 0 V; the scanning rate of CV is 10-100 mV / s.
[0012] The beneficial effects of the present invention are: rubber magnetic freezing shearing crushing, iron oxide powder magnetic separation calcination recovery, rubber carbon-activation preparation of porous carbon. The rubber and iron oxide magnetic powder are separated by liquid nitrogen freezing coupled with high-speed shearing, and the magnetic iron oxide is transferred by magnet, and repeated 3-5 times until there is no obvious iron oxide particle adsorbed on the magnet surface, thereby achieving effective separation of rubber and magnetic powder; the iron oxide can be reused after calcination, and the rubber can be carbonized-activated at high temperature to prepare porous carbon for supercapacitor electrode materials. This method can effectively realize the secondary utilization of rubber magnets and turn waste into treasure. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 These are scanning electron microscope photos of the porous carbons of Examples 1-5 of the present invention.
[0014] Figure 2 This is a transmission electron microscope photograph of the porous carbon prepared in Example 4 of the present invention.
[0015] Figure 3 This is the XRD curve of the porous carbon prepared in Example 4 of the present invention.
[0016] Figure 4 This is the Raman curve of the porous carbon prepared in Example 4 of the present invention.
[0017] Figure 5 This is the XPS curve of the porous carbon prepared in Example 4 of the present invention.
[0018] Figure 6 The electrochemical performance curves of the porous carbon prepared in Examples 1-5 of the present invention.
[0019] Figure 7The electrochemical performance comparison curve of the porous carbon prepared by Example 4 of the present invention and Comparative Examples 1-2 is shown. DETAILED DESCRIPTION
[0020] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific implementation methods. The present invention will be further described by examples, but is not limited to the following examples.
[0021] After 10 g of waste rubber magnets were placed in a liquid nitrogen tank for 5 min, they were transferred to a high-speed crusher and crushed for 30 min. The flaked ferrite magnetic powder was separated by adsorption with a magnet. The operation was repeated three times until there was no obvious adsorption of magnetic powder particles. The magnetic powder particles were used again after air calcination. The rubber particles were separated for the preparation of porous carbon.
[0022] The electrode preparation and testing process is as follows. This method is used in the implementation cases, so only the porous carbon preparation conditions are discussed in the cases. Porous carbon, PVDF, and conductive agent are mixed in a mass ratio of 8:1:1, and a small amount of N-methylpyrrolidone is added to grind into a paste, and evenly coated on 1×1 cm2 nickel foam, placed in an oven at 80 ºC to dry the pressed sheet; during the test, Hg / HgO and Pt sheets are used as reference electrodes and counter electrodes, porous carbon @ nickel foam is used as the working electrode, and 6 M potassium hydroxide aqueous solution is used as the electrolyte. The electrochemical test mainly includes cyclic voltammetry (CV) and constant current charge and discharge (GCD).
[0023] Implementation Case 1
[0024] The separated rubber particles were pre-carbonized at 250°C for 1 h to remove the volatile components on the surface, mixed with potassium hydroxide in a mass ratio of 1:1 and placed in a nickel crucible. A proper amount of alcohol was added and stirred evenly to dry. Finally, they were placed in a horizontal tube furnace under an inert atmosphere at 600°C for 1 h. After cooling to room temperature, they were washed with dilute hydrochloric acid and deionized water until neutral.
[0025] Implementation Case 2
[0026] The separated rubber particles were pre-carbonized at 250 ºC for 1 h to remove the volatile components on the surface, then mixed with potassium hydroxide in a mass ratio of 1:4 and placed in a nickel crucible. A proper amount of alcohol was added and stirred evenly to dry. Finally, the particles were placed in a horizontal tube furnace at 900 ºC for 2 h under an inert atmosphere. After cooling to room temperature, they were washed with dilute hydrochloric acid and deionized water until neutral.
[0027] Implementation Case 3
[0028] The separated rubber particles were pre-carbonized at 250 ºC for 1 h to remove the volatile components on the surface, mixed with potassium hydroxide in a mass ratio of 1:2 and placed in a nickel crucible. A proper amount of alcohol was added and stirred evenly to dry. Finally, the particles were placed in a horizontal tube furnace and treated at 800 ºC for 0.5 h under an inert atmosphere. After cooling to room temperature, they were washed with dilute hydrochloric acid and deionized water until neutral.
[0029] Implementation Case 4
[0030] The separated rubber particles were pre-carbonized at 250 ºC for 1 h to remove the volatile components on the surface, mixed with potassium hydroxide in a mass ratio of 1:2 and placed in a nickel crucible. A proper amount of alcohol was added and stirred evenly to dry. Finally, the particles were placed in a horizontal tube furnace and treated at 800 ºC for 1 h under an inert atmosphere. After cooling to room temperature, they were washed with dilute hydrochloric acid and deionized water until neutral.
[0031] Implementation Case 5
[0032] The separated rubber particles were pre-carbonized at 250 ºC for 1 h to remove the volatile components on the surface, mixed with potassium hydroxide in a mass ratio of 1:2 and placed in a nickel crucible. A proper amount of alcohol was added and stirred evenly to dry. Finally, the particles were placed in a horizontal tube furnace and treated at 800 ºC for 2 h under an inert atmosphere. After cooling to room temperature, they were washed with dilute hydrochloric acid and deionized water until neutral.
[0033] Comparative Case 1
[0034] The separated rubber particles were pre-carbonized at 350 ºC for 1 h to remove the volatile components on the surface, then mixed with potassium hydroxide in a mass ratio of 1:2 and placed in a nickel crucible. A proper amount of alcohol was added and stirred evenly to dry. Finally, the particles were placed in a horizontal tube furnace and treated at 800 ºC for 2 h under an inert atmosphere. After cooling to room temperature, they were washed with dilute hydrochloric acid and deionized water until neutral.
[0035] Comparative Case 2
[0036] The separated rubber particles were pre-carbonized at 250°C for 1 h to remove the volatile components on the surface, mixed with sodium hydroxide in a mass ratio of 1:2 and placed in a nickel crucible. A proper amount of alcohol was added and stirred evenly to dry. Finally, they were placed in a horizontal tube furnace under an inert atmosphere at 800°C for 1 h. After cooling to room temperature, they were washed with dilute hydrochloric acid and deionized water until neutral.
[0037] Figure 1Scanning electron microscope photos of porous carbon (a) Examples 1-5; (b) Example 2; (c) Example 3; (d) Example 4; (e) Example 5 (scale 20 μm, using JSM-700 field emission scanning electron microscope, test conditions: acceleration voltage 5.0 ~ 10.0 kV, vacuum degree 10-5 Pa). From the figure, it can be seen that the porous carbons prepared under different carbonization-activation conditions are all irregular micron particles, and the particle surface is relatively smooth, indicating that there are no obvious macropores.
[0038] Figure 2 This is a transmission electron microscope photo of the porous carbon prepared in Example 4 of the present invention (using a JEM-2010 high-resolution transmission electron microscope, test conditions: acceleration voltage 5.0 ~ 10.0 kV, vacuum degree 10-5 Pa). The porous carbon is in a disordered state as a whole, and mesopores can be clearly observed in the edge band.
[0039] Figure 3 This is the XRD curve of the porous carbon prepared in Example 4 of the present invention (using a D8 X-ray diffractometer, testing conditions: radiation source Cu Kα (λ = 0.15418nm)). The curve shows two obvious peaks, corresponding to the 002 (25°) and 100 peaks (41°) of the porous carbon, and there is no characteristic peak of iron oxide, indicating that the iron is completely removed after pickling.
[0040] Figure 4 This is the Raman curve of the porous carbon prepared in Example 4 of the present invention (using Nanofinder 3.0 spectrometer, test conditions: laser wavelength 488 nm). The curve shows two obvious peaks at 1350 and 1580 cm-1, corresponding to the D band and G band of the porous carbon respectively; 2700 cm-1 represents the 2D peak of the carbon material, which is mainly due to the residual iron catalyzing the rubber-based porous carbon to form more graphite microcrystalline areas; no iron peak was detected in the Raman peak, indicating that the iron was completely removed.
[0041] Figure 5 This is the XPS curve of the porous carbon prepared in Example 4 of the present invention (using AXIS Ultra DLD X-ray photoelectron spectrometer, test conditions: X-ray source is Mg Kα (1486.6 eV), power is 200 W). Three peaks of C, O and S can be observed from the curve, indicating that the porous carbon is composed of three elements of C, O and S, among which the introduction of O and S can increase the wettability of the electrode and the additional pseudocapacitance.
[0042] Figure 6 CV curves of porous carbon prepared in Examples 1-5 of the present invention (Shanghai Chenhua CHI760E) (a) 10 mVs-1 ; (b) 100 mV s -1 From the curve, it can be seen that the obtained carbon materials all show good rectangularity, indicating that the capacitance mechanism is mainly based on double-layer adsorption.
[0043] Figure 7 CV curves of porous carbon prepared in Example 4 of the present invention and Comparative Examples 1-2 (a) 10 mV s -1 ; (b) 100 mV s -1 ; (c) 10 mV s -1 ; (d) 100 mV s -1 ; GCD curve (e) 1 Ag -1 ; (f) 10 A g -1 From the CV curve, it can be seen that the potassium hydroxide activated carbon materials all show good rectangularity, indicating that the capacitance mechanism is mainly based on double-layer adsorption; while the sodium hydroxide activated carbon materials have poor rectangularity, mainly due to the retention of a large number of heteroatoms. GCD calculation shows that at 1A g -1 The specific capacitance of the three is between 170-200F g -1 Between 10A g -1 The specific capacitance is about 125-175F g -1 .
Claims
1. A method for magnetic separation and recovery of waste rubber and preparation of rubber-derived porous carbon electrode materials, characterized in that The following steps are included: (1) Separation of rubber and magnetic powder in rubber magnets: 10 g of waste rubber magnets were placed in a liquid nitrogen tank for 5 min, then transferred to a high-speed crusher for 30 min, and the detached ferrite magnetic powder was separated by adsorption using a magnet. The operation was repeated several times until no obvious magnetic powder particles were adsorbed. The magnetic powder particles were calcined in air and reused. (2) The separated rubber particles are pre-carbonized at 250-350°C for 1 h to remove the volatile components on the surface, and then mixed with an activator in a mass ratio of 1:1-1:4 and placed in a nickel crucible. A proper amount of alcohol is added and stirred to dry. Finally, the particles are placed in a horizontal tube furnace and treated at 600-900°C for 0.5-2 h under an inert atmosphere. After cooling to room temperature, they are washed with dilute hydrochloric acid and deionized water until neutral. (3) The porous carbon, PVDF binder and conductive agent obtained in step 2 were mixed in a mass ratio of 8:1:1, and a small amount of N-methylpyrrolidone was added to grind into a paste, and then evenly coated on 1×1 cm2 nickel foam, placed in an oven at 80 ºC to dry the pressed sheet for subsequent testing; (4) During the test, Hg / HgO and Pt sheets were used as reference electrodes and counter electrodes, porous carbon@nickel foam was used as the working electrode, and 6 M potassium hydroxide aqueous solution was used as the electrolyte. The electrochemical tests mainly included cyclic voltammetry (CV), constant current charge and discharge (GCD) and electrochemical impedance spectroscopy.
2. The method for magnetic separation and recovery of waste rubber and preparation of rubber-derived porous carbon electrode materials according to claim 1, characterized in that: The activator comprises potassium hydroxide and sodium hydroxide, the conductive agent is conductive carbon black or acetylene black, and the porous carbon loading on the nickel foam is 2 to 5 mg / cm2.
3. The method for magnetic separation and recovery of waste rubber and preparation of rubber-derived porous carbon electrode materials according to claim 1, characterized in that: The voltage window of the electrochemical test was -1 to 0 V; the scan rate of the CV was 10-100 mV / s.
Citation Information
Patent Citations
Method for preparing activated carbon by utilizing waste tire rubber
CN101708841A
Ferrite magnetic rubber magnetic powder recovery method
CN110126132A
Recovery of rubber
GB1334718A
Rubber and wire separation apparatus of recapped tire
KR101215444B1
Magnetic filtration process, magnetic filtering material, and methods of forming magnetic filtering material
US20100155335A1