Preparation method of micro-nano high-purity spherical silica powder

Through the combination of quartz mineralogical characteristics and high-temperature soft melting characteristics, combined with quartz purification, ultrafine grinding, chemical impurity removal and plasma technology, the problem of difficult to meet the particle size uniformity, sphericality and purity of silicon powder in the prior art is solved, and the problem of simultaneously meeting the uniformity of silicon powder particles in the existing technology is realized. The preparation of silicon micropowder with high purity, uniform particle size and high spherical shape has green and low consumption and large-scale industrial application potential.

CN118929672APending Publication Date: 2024-11-12CENT SOUTH UNIV

Patent Information

Application Number
CN202411090344.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing silicon micropowder preparation process is difficult to meet the requirements of uniform particle size, high spherical shape and high purity, especially in the submicron and nanoscale ranges. The existing methods are costly and complex in the process, so they cannot effectively meet the high-end fields. Demand for purity above level 4N.

Method used

Using quartz mineralogical characteristics and high-temperature soft melting characteristics, combined with the tandem synergistic effect of quartz purification, ultrafine grinding, chemical impurity removal and plasma technology, the high spherical shape is achieved through ultrafine grinding, chemical impurity removal and plasma high-temperature treatment. Preparation of silicon micropowders with high spherical morphology, small particle size and uniform particle size distribution, the purity of silicon micropowder can reach level 4N or above.

Benefits of technology

The preparation of silicon micropowder with high purity, uniform particle size and high spherical shape has been achieved, which reduces production difficulty and energy consumption, has green and low-cost process, strong applicability, and has the potential for large-scale industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929672A_ABST
    Figure CN118929672A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of micro-nano high-purity spherical silica powder, which comprises the following steps of: performing superfine grinding on a product obtained by crushing, grinding and physically sorting natural quartz ore and / or a fine-grained byproduct in a high-purity quartz sand production process to micro-nano level, and then sequentially performing chemical impurity removal and plasma high-temperature treatment, thereby obtaining the micro-nano high-purity spherical silica powder. The micro-nano grade 4N5 grade or above spherical silica powder is obtained. The method can be used for synchronously purifying the quartz sand and controlling the particle size and the sphericity degree, and has the advantages of simple production process, low chemical reagent consumption, uniform product particle size, high purity, high sphericity degree and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing micro-nano-level high-purity spherical silicon powder, belonging to the technical field of silicon dioxide preparation. Background Art

[0002] Under the background of the rapid development of science and technology, spherical silicon micropowder has shown great market potential due to its unique properties and wide applications, especially in the fields of large-scale integrated circuit packaging, aviation, aerospace, fine chemicals, rewritable optical disks, large-area electronic substrates, special ceramics and daily cosmetics. However, existing production processes such as flame method and high-temperature melt spraying method face challenges in preparing submicron and nanometer spherical silicon micropowders with uniform particle size, and it is often difficult to achieve ideal size control. For example, Chinese patent CN101037206A discloses a method for obtaining spherical silicon micropowder by centrifugal spray drying and plasma flame heat treatment of silica sol. This method can obtain high-quality spherical silicon micropowder with high spheroidization rate, high sphericity, high density and good surface smoothness, but the particle size of the silicon micropowder obtained by this method is micron-level and the purity of the silicon micropowder cannot be improved simultaneously.

[0003] Submicron (0.1-1μm) and nanometer (1-100nm) spherical silicon powders are considered to be important materials for the future due to their superior performance and wide range of uses, but their preparation process is complex and costly. For example, the method of generating submicron spherical silicon powders by reacting specific silicon source compounds with oxygen under flame or suitable temperature conditions can produce the desired products, but there are cumbersome steps and economic pressures in the raw material preparation and subsequent processing.

[0004] In addition, the purity of spherical silicon micropowder is crucial to its performance in high-end fields such as semiconductors, electronics, and optics. Applications in these fields usually require 4N or even higher purity silicon micropowder to ensure effective support, protection, and stable operation of electronic components. However, the current mainstream physical preparation methods, such as flame method, high-temperature melt spray method, and plasma method, are limited by process conditions and can only produce 2N to 3N grade spherical silicon micropowder. Although high-purity silicon micropowder can be obtained through silicon-based organic compounds combined with hydrothermal, precipitation, microemulsion and other chemical methods, this brings a lot of reagent consumption and safety hazards.

[0005] In view of this, extracting from natural minerals and developing a green and efficient production process that can mass-produce micro-nano-scale and high-purity spherical silicon powder is not only of great significance for meeting the demand for high-end silicon-based materials, but will also play a key role in promoting the sustainable development of the entire industry. Summary of the invention

[0006] In view of the problems existing in the existing technology for preparing silicon micropowder, such as being unable to simultaneously meet the requirements of product purity, particle size and sphericity, the purpose of the present invention is to provide a method for preparing micro-nano-level high-purity spherical silicon micropowder. The method is based on the mineralogical properties and high-temperature soft melting characteristics of quartz, combined with the advantages of quartz purification, ultrafine grinding, chemical impurity removal and plasma technology and the series synergistic effect between the processes, to achieve the preparation of silicon micropowder with high sphericity, high sphericity rate, small particle size and uniform particle size distribution, and the purity of the silicon micropowder can reach above 4N level.

[0007] In order to achieve the above technical objectives, the present invention provides a method for preparing micro-nano-level high-purity spherical silicon powder, which comprises the following steps: ultrafine grinding the products of crushing, grinding and physical separation of natural quartz ore and / or the fine-grained byproducts of the high-purity quartz sand production process to micro-nano-level, and then subjecting them to chemical impurity removal and plasma high-temperature treatment in sequence, so as to obtain micro-nano-level 4N5-level or higher spherical silicon powder; the conditions for the plasma high-temperature treatment are: temperature ≥5000K and material residence time of 0.5 to 3 min.

[0008] The key to the technical solution of the present invention lies in the synergistic effect between ultrafine grinding, chemical impurity removal and plasma high temperature treatment processes. First, by selecting quartz raw materials with higher SiO2 purity, the production difficulty and energy consumption of subsequent processes can be reduced. Secondly, the ultrafineness of the raw material particle size is the key to the physical method of producing high-purity ultrafine spherical silicon micropowder. The impurity components in the quartz raw materials of the present invention mainly include surface adhesion impurities and impurities coated inside the particles. Therefore, the present invention can fully expose the impurities inside the quartz particles by adopting ultrafine grinding to micro-nano level, which is conducive to the subsequent impurity removal process. However, ultrafine grinding inevitably adheres the grinding material to the surface of the quartz powder, and lattice impurities are still left inside the quartz and are not removed. Therefore, the present invention performs chemical impurity removal on the quartz after ultrafine grinding, which further improves the purity of the silicon micropowder in depth. However, the quartz material still has an irregular morphology after the above-mentioned process treatment. In order to obtain products with high sphericity and high spheroidization rate, the above-mentioned high-purity quartz powder needs to be morphologically adjusted. Finally, the present invention can make high-purity quartz powder quickly remelt by adopting plasma high-temperature treatment, adjust the high-temperature holding time of the material, make it fully spherical, and avoid the remelted quartz powder from sticking to each other while maintaining the high purity of quartz sand.

[0009] The technical solution of the present invention has a wide range of raw material selection, which can be used for both natural quartz ore and fine-grained by-products of the production process of high-purity quartz sand. For natural quartz ore, the present invention is based on the occurrence morphology, embedding relationship, and cleavage surface characteristics of quartz ore phases and associated minerals, and realizes the dissociation of quartz ore phases and associated minerals along the ore phase interface through precise crushing and grinding processes, thereby improving the dissociation effect of different ore phases. According to the differences in the chemical composition, density, and electromagnetic characteristics of associated minerals, gravity separation, magnetic separation, electric separation, color separation, and flotation separation are selected to separate quartz minerals from associated minerals, thereby obtaining quartz concentrates with high recovery rates and purity as raw materials for subsequent processing. In addition, a large number of fine-grained quartz particles or defective products in the production process of high-purity quartz products such as quartz sand for crucibles will be produced during the production process. These quartz products have high purity and can also be used as raw materials for the production of high-purity micro-nano spherical silicon powder of the present invention, which is helpful to improve the high-value utilization of all components of quartz raw materials in high-purity quartz product manufacturers such as quartz sand for crucibles.

[0010] Rapid ultra-high temperature treatment is the key to the spheroidization of ultra-fine quartz powder. In this process, the quartz powder is quickly softened, and the soft-melted quartz powder is separated from the ultra-high temperature environment before dripping or sticking, so that it condenses. This process can achieve the spheroidization of particles. Rapid high-temperature heating and high-temperature holding time are the key to obtaining products with high sphericity and high spheroidization rate. The inventors found that according to the characteristics of the quartz crystal structure and the energy storage characteristics of ultra-fine quartz powder, when the temperature is lower than 5000K, the spheroidization rate of quartz particles is low; when the temperature is ≥5000K, the high-temperature residence time exceeds 3min, which will lead to significant dripping and droplet aggregation.

[0011] As a preferred solution, the physical separation includes at least one of gravity separation, magnetic separation, electric separation, color separation and flotation.

[0012] As a preferred solution, the product of the crushing, grinding and physical separation is a quartz concentrate with a SiO2 content of ≥99.5%.

[0013] As a preferred solution, the fine-grained by-product is the screened material and / or defective product in the production process of quartz sand of grade 4N or above, and the SiO2 content is ≥99.5%.

[0014] As a preferred solution, the natural quartz ore is at least one of vein quartz, quartzite and pegmatite.

[0015] As a preferred solution, the ultrafine grinding is at least one of high-energy ball milling, nano-milling and air flow milling.

[0016] As a preferred solution, the micro-nano level has a particle size of ≤1 μm. Ultrafine particle size is a prerequisite for preparing micro-nano high-purity spherical silicon powder. Conventional grinding technologies such as ball milling, rod milling, roller milling, etc. can obtain quartz powder with a particle size of ≤1 μm, but the yield of this particle size is not high, and repeated screening is required to obtain related products, resulting in low production efficiency and high labor intensity. The high-energy ball mill, nano-grinding and air flow mill preferred by the present invention have the advantages of high finished product fineness, moderate processing scale, and continuous production, and can be used to obtain ultrafine quartz powder in batches. In addition, the above-mentioned ultrafine grinding process has the advantages of simple particle size control and can meet the production of products of different particle size grades. The particle size of quartz sand also has a direct impact on the impurity removal and subsequent sphericity of quartz sand. When the particle size of quartz sand is large, not only will the impurities inside the quartz sand not be fully exposed, reducing the purification effect, but it will also lead to a low degree of soft melting during the high-temperature plasma treatment process, which in turn leads to a low degree of sphericity, reducing the product particle size and sphericity.

[0017] As a preferred solution, the chemical impurity removal is at least one of acid leaching, alkali leaching, salt leaching and roasting, and the chemical impurity removal controls the SiO2 content in the quartz sand to be ≥99.995%. The acid leaching, alkali leaching and salt leaching of the present invention are to remove impurities adhering to the surface of the quartz powder or coated on the quartz particles, while roasting can further deeply remove impurities coated on the quartz particles or lattice impurities, thereby achieving deep purification of the quartz powder. It is further preferred to use at least one of acid leaching, alkali leaching and salt leaching in combination with roasting to increase the SiO2 content to above 5N level.

[0018] As a preferred solution, the acid leaching uses at least one of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and oxalic acid as the leaching medium; the alkaline leaching uses sodium hydroxide and / or potassium hydroxide as the leaching medium; the salt leaching uses ammonium chloride and / or ammonium sulfate as the leaching medium; the conditions of the acid leaching, alkaline leaching and salt leaching are: the concentration of the leaching agent is 0.5-2 mol / l, the liquid-solid ratio is (1-3):1, the leaching time is 30-90min, and the temperature is 25-80°C. Under the preferred conditions of the present invention, an efficient and low-consumption impurity removal process can be achieved. Since the quartz material to be leached is an ultrafine powder with fine particle size and low impurity content, high reagent concentration, long leaching time and high temperature can achieve sufficient dissolution and removal of impurities, but it is inevitable to cause partial dissolution of quartz powder. On the contrary, although the dissolution of quartz powder can be reduced, it will cause problems such as incomplete removal of impurities.

[0019] As a preferred solution, the calcination conditions are: using at least one of air, HCl, Cl2, H2 and CO as the calcination atmosphere, the flow rate of the calcination atmosphere is 3-8 ml / min, the temperature is 800-1100°C, and the time is 5-20 min. High calcination temperature, long calcination time, and large calcination gas flow rate are beneficial to the removal of lattice impurities, but they will inevitably cause partial softening of ultrafine quartz powder or consolidation of particles, resulting in increased particle size and other problems. On the contrary, it will lead to incomplete removal of lattice impurities.

[0020] As a preferred solution, the roasting includes at least one of chlorination roasting, air roasting and reduction roasting.

[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:

[0022] 1) Based on the mineralogical properties and high-temperature soft melting characteristics of quartz, the present invention combines the advantages of quartz purification, ultrafine grinding, chemical impurity removal and plasma technology and the series synergistic effect between the processes to achieve the preparation of silicon micropowder with high sphericity, high sphericity rate, small particle size and uniform particle size distribution. At the same time, the purity of the silicon micropowder can reach above 4N level.

[0023] 2) The production process of the present invention does not use silicon-based organic reagents, and the production process has little impact on operators and the ecological environment, and has the technical advantages of being green and low-consumption.

[0024] 3) The raw materials of the present invention have a wide range of sources, and can be obtained by processing natural minerals, or fine-grained powder or defective products in the production process such as high-purity quartz sand, and the raw materials have strong applicability.

[0025] 4) The process equipment used in the present invention is highly mature and has a variety of equipment selections, which can meet the production of different regions and different target products. It has strong operability and has the potential for large-scale industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the morphology of the micro-nano-level high-purity spherical silicon powder product prepared by the preparation method of the present invention. DETAILED DESCRIPTION

[0027] In order to facilitate the understanding of the present invention, the present invention will be described in more comprehensive and detailed manner in conjunction with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0028] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0029] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.

[0030] Example 1

[0031] The vein quartz is crushed and ground to a particle size of ≤1mm by a jaw crusher and a ball mill, and the associated mineral impurities are removed by gravity separation and magnetic separation to obtain a quartz concentrate with a SiO2 content of ≥99.5%. The quartz concentrate is ultra-finely refined to a particle size of <1μm by a jet mill, and acid leached with 1mol / l HCl, a liquid-solid ratio of 2:1, a leaching time of 45min, and a temperature of 80°C. The obtained samples are washed and dried and then used for plasma high-temperature treatment at a temperature of 5000K and a high-temperature residence time of 3min. The test results show that the product has an SiO2 content of 99.996%, a particle size of 600-900nm, a sphericity≈1, and a spheroidization rate of 98.9%.

[0032] Example 2

[0033] The quartzite is crushed and ground by impact crusher and rod mill to a particle size of less than 0.9 mm, and the associated mineral impurities are removed by magnetic separation and flotation to obtain a quartz concentrate with a SiO2 content of ≥99.9%. The quartz concentrate is refined by high-energy ball milling to a particle size of less than 1 μm, and is acid-leached with a mixed acid of HCl and HF (the volume ratio of HCl and HF is 1:1) with a total concentration of 0.5 mol / l, a liquid-solid ratio of 1:1, a leaching time of 30 minutes, and a temperature of 25°C. The quartz concentrate is then chlorinated and roasted at a roasting temperature of 1100°C, an HCl flow rate of 3 ml / min, and a roasting time of 5 minutes. The obtained sample is used for plasma high-temperature treatment at a temperature of 8000K and a high-temperature residence time of 0.5 minutes. The test results show that the product has a SiO2 content of 99.9996%, a particle size of 500-750 nm, a sphericity of ≈1, and a spheroidization rate of 99.3%.

[0034] Example 3

[0035] The vein quartz is crushed and ground to a particle size of less than 0.9 mm by a cone crusher and a rod mill, and the associated mineral impurities are removed by magnetic separation and flotation to obtain a quartz concentrate with a SiO2 content of ≥99.96%. The quartz concentrate is refined to a particle size of less than 1 μm by nano-grinding, and salt leached with 2 mol / l ammonium chloride, a liquid-solid ratio of 3:1, a leaching time of 90 min, and a temperature of 60°C. The concentrate is then air roasted at a temperature of 800°C and a roasting time of 20 min. The obtained sample is used for plasma high-temperature treatment at a temperature of 7600K and a high-temperature residence time of 2 min. The test results show that the product has a SiO2 content of 99.9991%, a particle size of 500-800 nm, a sphericity of ≈1, and a spheroidization rate of 99.1%.

[0036] Example 4

[0037] The pegmatite was crushed and ground by impact crusher and roller mill to a particle size of less than 1 mm, and the associated mineral impurities were removed by color sorting, magnetic separation and flotation to obtain a quartz concentrate with a SiO2 content of ≥99.94%. The quartz concentrate was refined by nano-grinding to a particle size of less than 1 μm, and alkaline leaching was carried out using 1 mol / l NaOH with a liquid-to-solid ratio of 1:1, a leaching time of 30 min, and a temperature of 40°C. The quartz concentrate was then reduced and roasted with hydrogen at a roasting temperature of 1000°C, a gas flow rate of 8 ml / min, and a roasting time of 10 min. The obtained sample was used for plasma high-temperature treatment at a temperature of 9300 K and a high-temperature residence time of 1 min. The test results showed that the product had an SiO2 content of 99.9993%, a particle size of 50-110 nm, a sphericity of ≈1, and a spheroidization rate of 99.7%.

[0038] Example 5

[0039] The fine-grained material with a particle size of less than 0.1 mm in the production process of high-purity quartz sand is used for flotation to remove associated mineral impurities to obtain a quartz concentrate with a SiO2 content of ≥99.96%. The quartz concentrate is refined to a particle size of less than 1 μm by nano-grinding, and acid leaching is carried out with hydrochloric acid and oxalic acid with a total concentration of 1 mol / l (the volume ratio of hydrochloric acid to oxalic acid is 1:1), a liquid-solid ratio of 1:1, a leaching time of 25 minutes, and a temperature of 40°C. Chlorine is then used for chlorination roasting at a roasting temperature of 900°C, a gas flow rate of 5 ml / min, and a roasting time of 10 minutes. The obtained sample is used for plasma high-temperature treatment at a temperature of 9000K and a high-temperature residence time of 1 minute. The test results show that the product has a SiO2 content of 99.9993%, a particle size of 700-900 nm, a sphericity of ≈1, and a spheroidization rate of 99.3%.

[0040] Comparative Example 1

[0041] Compared with Example 1, the only difference is that the ultrafine quartz powder is not subjected to acid leaching treatment.

[0042] The final product has a SiO2 content of 99.4%, a particle size of 600-900nm, a sphericity of ≈1, and a spheroidization rate of 96.4%.

[0043] Comparative Example 2

[0044] Compared with Example 2, the only difference is that the quartz concentrate is subjected to high-energy ball milling treatment, but the particle size is less than 100 μm and greater than 50 μm.

[0045] The final product has a SiO2 content of 99.97%, a particle size of 147-861 μm, a sphericity of ≈0.8, and a spheroidization rate of 63.5%.

[0046] Comparative Example 3

[0047] Compared with Example 4, the only difference is that the plasma treatment temperature is 3700K.

[0048] The final product has a SiO2 content of 99.9991%, a particle size of 600-800nm, a sphericity of ≈0.6, and a spheroidization rate of 47.1%.

[0049] Comparative Example 4

[0050] Compared with Example 5, the difference is that the quartz concentrate obtained by flotation is acid leached, chlorinated and roasted, then nano-grinded, and then subjected to plasma high-temperature treatment. The above process parameters are the same as those in Example 5.

[0051] The final product has a SiO2 content of 99.993%, a particle size of 700-900 nm, a sphericity of ≈0.9, and a spheroidization rate of 97.6%. From the data comparison of Comparative Example 4 and Example 5, it can be seen that the present invention can only be deeply purified by subsequent chemical impurity removal only after the impurities inside the quartz sand particles are exposed by nano-grinding, and the effect of the subsequent plasma high temperature treatment is also affected to a certain extent.

Claims

1. A method for preparing micro-nano high-purity spherical silicon powder, characterized in that: The products of crushing, grinding and physical separation of natural quartz ore and / or the fine-grained by-products of the high-purity quartz sand production process are ultrafinely ground to micro-nano level and then subjected to chemical impurity removal and plasma high-temperature treatment in sequence to obtain spherical silicon micropowder of micro-nano level 4N5 or above; the conditions of the plasma high-temperature treatment are: temperature ≥5000K and material residence time of 0.5 to 3 minutes.

2. The method for preparing micro-nano high-purity spherical silicon powder according to claim 1, characterized in that: The product of the crushing, grinding and physical separation is a quartz concentrate with a SiO2 content of ≥99.5%; The fine-grained by-product is the screened material and / or defective product in the production process of quartz sand above grade 4N, and the SiO2 content is ≥99.5%.

3. The method for preparing micro-nano high-purity spherical silicon powder according to claim 1, characterized in that: The natural quartz ore is at least one of vein quartz, quartzite and pegmatite.

4. A method for preparing micro-nano high-purity spherical silicon powder according to any one of claims 1 to 3, characterized in that: The ultrafine grinding is at least one of high energy ball grinding, nano grinding and air flow grinding.

5. The method for preparing micro-nano high-purity spherical silicon powder according to claim 4, characterized in that: The micro-nano level refers to a particle size ≤ 1 μm.

6. The method for preparing micro-nano high-purity spherical silicon powder according to claim 5, characterized in that: The chemical impurity removal is at least one of acid leaching, alkali leaching, salt leaching and roasting.

7. The method for preparing micro-nano high-purity spherical silicon powder according to claim 6, characterized in that: The acid leaching uses at least one of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and oxalic acid as the leaching medium; the alkali leaching uses sodium hydroxide and / or potassium hydroxide as the leaching medium; the salt leaching uses ammonium chloride and / or ammonium sulfate as the leaching medium; the conditions of the acid leaching, alkali leaching and salt leaching are: the concentration of the leaching agent is 0.5-2 mol / l, the liquid-solid ratio is (1-3):1, the leaching time is 30-90 min, and the temperature is 25-80°C.

8. The method for preparing micro-nano high-purity spherical silicon powder according to claim 6, characterized in that: The calcination conditions are: using at least one of air, HCl, Cl2, H2 and CO as the calcination atmosphere, the flow rate of the calcination atmosphere is 3-8 ml / min, the temperature is 800-1100° C., and the time is 5-20 min.

Citation Information

Patent Citations

  • Production method of active high-purity nanoscale crystal silicon micro-powder

    CN108609625A

  • Preparation method of high-activity spherical calcined coal gangue powder

    CN113860780A

  • Method of production of the high-structured carbon-mineral composites produced out of the high-ash biomass

    RU2310602C1

Cited By

  • Method for directionally removing impurity elements of pegmatite type high-purity quartz

    CN119569068A

  • Efficient and high-value utilization method of waste quartz crucible

    CN121269718A

  • Method for efficient and high-value utilization of waste quartz crucible

    CN121269718B

  • Nanoscale spherical silicon powder as well as preparation method and application thereof

    CN122464428A