Cerium modified Cu-SSZ-13 molecular sieve and preparation method thereof

By preparing cerium modified Cu-SSZ-13 molecular sieve, the problem of insufficient efficiency in removing NH3/Hg0 pollutants was solved, and the ammonia and mercury oxidation properties of the catalyst were improved, especially in It exhibits higher activity and selectivity under low temperature conditions.

CN118929690APending Publication Date: 2024-11-12NORTH CHINA ELECTRIC POWER UNIV

Patent Information

Application Number
CN202411164656.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing cerium-based Cu-SSZ-13 catalysts are inefficient in removing NH3/Hg0 contaminants, and their low-temperature activity is significantly reduced especially in the presence of sulfur dioxide.

Method used

A method of preparing cerium-modified Cu-SSZ-13 molecular sieve is adopted, by mixing materials such as sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, etc., crystallization and calcining, and then doping using an aluminum ion source. , Ce(NO3)3·6H2O and hexamethylenetetramine were added to the aqueous ethanol solution, and a cerium-modified Cu-SSZ-13 molecular sieve was obtained after multiple calcination.

Benefits of technology

The removal efficiency of NH3/Hg0 pollutants by cerium modified Cu-SSZ-13 is significantly improved, and the ammonia oxidation activity and mercury oxidation properties of the catalyst are enhanced, especially under low temperature conditions, which show higher activity and selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929690A_ABST
    Figure CN118929690A_ABST
Patent Text Reader

Abstract

The invention discloses a cerium modified Cu-SSZ-13 molecular sieve preparation method, which comprises: A, mixing sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate and benzyltrimethylamine with water to prepare a mixed gel, standing for 5 h in a 70 DEG C environment, and carrying out crystallization treatment; b, roasting the crystallized substance for the first time, doping the crystallized substance by using an aluminum ion source and adopting an ion implantation method, and roasting the crystallized substance for the second time to obtain a Cu-SSZ-13 molecular sieve; and C, crushing the Cu-SSZ-13 molecular sieve, adding the crushed Cu-SSZ-13 molecular sieve into an ethanol water solution, stirring, adding polyvinylpyrrolidone, Ce (NO3) 3.6 H2O and hexamethylenetetramine, stirring for 2 hours, refluxing for 2 hours at 60 DEG C, carrying out suction filtration, washing, drying, and roasting to obtain the cerium modified Cu-SSZ-13 molecular sieve. According to the method, the defects in the prior art can be overcome, and the removal efficiency of the cerium-based Cu-SSZ-13 on NH3 / Hg0 pollutants is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, in particular to a cerium-modified Cu-SSZ-13 molecular sieve and a preparation method thereof. Background Art

[0002] Molecular sieve catalysts are a type of catalytic material with high specific surface area, ordered pore structure and good stability, including SAPO-34, ZSM-5, SSZ-13, Y, Beta, etc. Among them, copper-based SSZ-13 molecular sieve (Cu-SSZ-13) is widely used in the removal of NH3 / Hg 0 However, sulfur dioxide can significantly reduce the low-temperature activity of Cu-SSZ-13, so in recent years, cerium-based Cu-SSZ-13 has gradually been developed to improve the tolerance of Cu-SSZ-13 to sulfur dioxide. However, the existing cerium-based Cu-SSZ-13 has poor tolerance to NH3 / Hg 0 The removal efficiency of pollutants needs to be improved. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a cerium-modified Cu-SSZ-13 molecular sieve and a preparation method thereof, which can solve the deficiencies of the prior art and improve the NH3 / Hg 0 Pollutant removal efficiency.

[0004] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows.

[0005] A method for preparing a cerium-modified Cu-SSZ-13 molecular sieve comprises the following steps:

[0006] A. Sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, and benzyltrimethylamine were mixed with water to prepare a mixed gel, which was allowed to stand at 70° C. for 5 hours and then subjected to crystallization treatment;

[0007] B. calcining the crystallized product for the first time, then doping the crystallized product by ion implantation using an aluminum ion source, and then calcining the crystallized product for the second time to obtain a Cu-SSZ-13 molecular sieve;

[0008] C. Crush the Cu-SSZ-13 molecular sieve, add it into an ethanol aqueous solution and stir it, then add polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine, stir it for 2 hours, reflux it at 60°C for 2 hours, filter it, wash it, dry it, and then roast it to obtain a cerium-modified Cu-SSZ-13 molecular sieve.

[0009] Preferably, in step A, the molar ratio of sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine and water is 1:60:1:23:12:150.

[0010] Preferably, in step A, the crystallization treatment adopts a steam-assisted crystallization method, the crystallization treatment temperature is 170° C., and the crystallization time is 24 hours.

[0011] Preferably, in step B, the temperature of the first calcination is 340° C., and the time of the first calcination is 6 h; the temperature of the second calcination is 650° C., and the time of the second calcination is 12 h.

[0012] Preferably, in step B, the aluminum ion source used for ion implantation is trimethylaluminum, the flow rate of the aluminum ion source is 80 sccm, the voltage is 30 kV, and the pressure is 1×10 -3 Pa~3×10 -3 Pa, processing time is 0.5h.

[0013] Preferably, in step C, the ethanol content of the ethanol aqueous solution is 60wt%, and the mass ratio of Cu-SSZ-13 molecular sieve, ethanol aqueous solution, polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine is 1:1200:10:3:2.

[0014] Preferably, in step C, the calcination temperature is 500°C and the calcination time is 12 hours.

[0015] A cerium-modified Cu-SSZ-13 molecular sieve is prepared using the above-mentioned method for preparing the cerium-modified Cu-SSZ-13 molecular sieve.

[0016] The beneficial effect brought about by adopting the above technical solution is that the cerium-modified Cu-SSZ-13 molecular sieve prepared by the present invention has obvious advantages in the oxidation treatment capacity of pollutants such as ammonia and mercury. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a comparison chart of the ammonia oxidation activity of each sample at different temperatures.

[0018] Figure 2 Comparison of nitrogen selectivity of each sample at different temperatures.

[0019] Figure 3 This is a comparison chart of the effect of NO on the ammonia oxidation efficiency of each sample at different temperatures.

[0020] Figure 4 Comparison of nitrogen selectivity of each sample at different temperatures.

[0021] Figure 5 This is a comparison chart of the denitrification performance of each sample at different temperatures.

[0022] Figure 6 This is a comparison chart of the mercury oxidation performance of each sample at different temperatures.

[0023] Figure 7 The figure is a comparison chart of mercury oxidation performance of each sample in the presence of ammonia at different temperatures.

[0024] Figure 8 This is a comparison chart of the ammonia oxidation performance of each sample in the presence of mercury at different temperatures.

[0025] Fig. 9 This is a comparison chart of the effect of SO2 on the ammonia oxidation efficiency of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 at 250°C.

[0026] Fig.10 This is a comparison of the effects of SO2 on the nitrogen selectivity of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 at 250°C.

[0027] Fig.11 This is a comparison chart of the effect of SO2 on the ammonia oxidation efficiency of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 in the presence of NO at 250°C.

[0028] Fig.12 This is a comparison chart of the effect of SO2 on the denitrification efficiency of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 at 250°C.

[0029] Fig.13 This is a comparison chart of the effect of SO2 on the nitrogen selectivity of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 in the presence of NO at 250°C.

[0030] Fig.14 This is a comparison chart of the effects of SO2 on mercury oxidation of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 at 250°C.

[0031] Fig.15 HR-TEM characterization results of Cu-SSZ-13@CeO2-2.

[0032] Fig.16 These are the N2 adsorption-desorption curves of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2.

[0033] Fig.17 This is the pore size distribution diagram of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2.

[0034] Fig.18 XRD patterns of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2.

[0035] Fig.19 XPS O 1s spectra of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2.

[0036] Fig. 20 XPS Cu 2p spectra of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2.

[0037] Fig.21 XPS Ce 3d spectra of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2.

[0038] Fig. 22 DRIFT spectra of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 after NH3 pretreatment for 30 min.

[0039] Fig.23 This is the DRIFT spectrum of NH3 pretreated Cu-SSZ-13 changing with time after O2 was introduced.

[0040] Fig.24 The DRIFT spectrum of Cu-SSZ-13@CeO2-2 pretreated with NH3 changes over time after the introduction of O2.

[0041] Fig.25 These are the mercury temperature-programmed desorption curves of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2. DETAILED DESCRIPTION

[0042] Example 1

[0043] A method for preparing a cerium-modified Cu-SSZ-13 molecular sieve comprises the following steps:

[0044] A. Sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, and benzyltrimethylamine are mixed with water to prepare a mixed gel, wherein the molar ratio of sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine and water is 1:60:1:23:12:150. The mixed gel is allowed to stand at 70°C for 5 hours and then subjected to crystallization treatment; the crystallization treatment adopts a steam-assisted crystallization method, the crystallization treatment temperature is 170°C, and the crystallization time is 24 hours.

[0045] B. The crystallized product is first calcined at a temperature of 340°C for 6 hours. Then, an aluminum ion source is used to dope the crystallized product by ion implantation. The aluminum ion source used for ion implantation is trimethylaluminum. The flow rate of the aluminum ion source is 80 sccm, the voltage is 30 kV, and the pressure is 1×10 -3 Pa~3×10 -3Pa, the treatment time is 0.5h. Then the crystallized product is calcined for the second time, the temperature of the second calcination is 650°C, the time of the second calcination is 12h, and the Cu-SSZ-13 molecular sieve is obtained.

[0046] C. Crush the Cu-SSZ-13 molecular sieve, add it into an ethanol aqueous solution and stir it, then add polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine, the ethanol content of the ethanol aqueous solution is 60wt%, and the mass ratio of Cu-SSZ-13 molecular sieve, ethanol aqueous solution, polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine is 1:1200:10:3:2. After stirring for 2h, reflux at 60°C for 2h, filter, wash, and dry, and then calcine at a temperature of 500°C for 12h to obtain a cerium-modified Cu-SSZ-13 molecular sieve (the molecular sieve prepared in this embodiment is recorded as Cu-SSZ-13@CeO2-2).

[0047] Comparative Example 1

[0048] A method for preparing Cu-SSZ-13 molecular sieve comprises the following steps:

[0049] Sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine were mixed with water to obtain a mixed gel, wherein the molar ratio of sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine and water was 1:60:1:23:12:150, and the mixture was allowed to stand for 5 hours at 70°C, and then crystallized; the crystallization was carried out by steam-assisted crystallization, the crystallization temperature was 170°C, and the crystallization time was 24h. The crystallized product was calcined at a temperature of 650°C and a calcination time of 16h to obtain a Cu-SSZ-13 molecular sieve (the molecular sieve obtained in this comparative example is recorded as Cu-SSZ-13).

[0050] Comparative Example 2

[0051] A method for preparing a cerium-modified Cu-SSZ-13 molecular sieve comprises the following steps:

[0052] Sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine and water were mixed to prepare a mixed gel, wherein the molar ratio of sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine and water was 1:60:1:23:12:150, and the mixed gel was allowed to stand at 70°C for 5 hours, and then crystallized; the crystallization was carried out by steam-assisted crystallization, the crystallization temperature was 170°C, and the crystallization time was 24 hours. The crystallized product was calcined at a temperature of 650°C and a calcination time of 16 hours.

[0053] The Cu-SSZ-13 molecular sieve is crushed and added to an ethanol aqueous solution for stirring. Then, polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine are added. The ethanol content of the ethanol aqueous solution is 60wt%, and the mass of Cu-SSZ-13 molecular sieve, ethanol aqueous solution, polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine is 1:1200:10:3:2. After stirring for 2h, reflux at 60°C for 2h. After suction filtration, washing and drying, calcination is performed at a temperature of 500°C and a calcination time of 12h to obtain a cerium-modified Cu-SSZ-13 molecular sieve (the molecular sieve prepared in this embodiment is recorded as Cu-SSZ-13@CeO2-1).

[0054] Comparative Example 3

[0055] A method for preparing a cerium-modified Cu-SSZ-13 molecular sieve comprises the following steps:

[0056] A. Sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, and benzyltrimethylamine are mixed with water to prepare a mixed gel, wherein the molar ratio of sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine and water is 1:60:1:23:12:150. The mixed gel is allowed to stand at 70°C for 5 hours and then subjected to crystallization treatment; the crystallization treatment adopts a steam-assisted crystallization method, the crystallization treatment temperature is 170°C, and the crystallization time is 24 hours.

[0057] B. The crystallized product is first calcined at a temperature of 340°C for 6 hours. Then, an aluminum ion source is used to dope the crystallized product by ion implantation. The aluminum ion source used for ion implantation is trimethylaluminum. The flow rate of the aluminum ion source is 80 sccm, the voltage is 30 kV, and the pressure is 1×10 -3 Pa~3×10 -3 Pa, the treatment time is 0.5h. Then the crystallized product is calcined for the second time, the temperature of the second calcination is 650°C, the time of the second calcination is 12h, and the Cu-SSZ-13 molecular sieve is obtained.

[0058] C. Crush the Cu-SSZ-13 molecular sieve, add it into an ethanol aqueous solution and stir it, then add polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine, the ethanol content of the ethanol aqueous solution is 60wt%, and the mass ratio of Cu-SSZ-13 molecular sieve, ethanol aqueous solution, polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine is 1:1200:10:4:2. After stirring for 2h, reflux at 60°C for 2h, filter, wash, and dry, and then calcine at a temperature of 500°C for 12h to obtain a cerium-modified Cu-SSZ-13 molecular sieve (the molecular sieve prepared in this embodiment is recorded as Cu-SSZ-13@CeO2-3).

[0059] Comparative Example 4

[0060] A method for preparing a cerium-modified Cu-SSZ-13 molecular sieve comprises the following steps:

[0061] A. Sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, and benzyltrimethylamine are mixed with water to prepare a mixed gel, wherein the molar ratio of sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine and water is 1:60:1:23:12:150. The mixed gel is allowed to stand at 70°C for 5 hours and then subjected to crystallization treatment; the crystallization treatment adopts a steam-assisted crystallization method, the crystallization treatment temperature is 170°C, and the crystallization time is 24 hours.

[0062] B. The crystallized product is first calcined at a temperature of 340°C for 6 hours. Then, an aluminum ion source is used to dope the crystallized product by ion implantation. The aluminum ion source used for ion implantation is trimethylaluminum. The flow rate of the aluminum ion source is 80 sccm, the voltage is 30 kV, and the pressure is 1×10 -3 Pa~3×10 -3 Pa, the treatment time is 0.5h. Then the crystallized product is calcined for the second time, the temperature of the second calcination is 650°C, the time of the second calcination is 12h, and the Cu-SSZ-13 molecular sieve is obtained.

[0063] C. The Cu-SSZ-13 molecular sieve was crushed, added into an ethanol aqueous solution and stirred, and then polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine were added, the ethanol content of the ethanol aqueous solution was 60wt%, and the mass ratio of Cu-SSZ-13 molecular sieve, ethanol aqueous solution, polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine was 1:1200:10:2:2. After stirring for 2h, the mixture was refluxed at 60°C for 2h, filtered, washed, and dried, and then calcined at 500°C for 12h to obtain a cerium-modified Cu-SSZ-13 molecular sieve (the molecular sieve prepared in this embodiment is recorded as Cu-SSZ-13@CeO2-4).

[0064] Comparative Example 5

[0065] A method for preparing a cerium-modified Cu-SSZ-13 molecular sieve comprises the following steps:

[0066] A. Sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, and benzyltrimethylamine are mixed with water to prepare a mixed gel, wherein the molar ratio of sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine and water is 1:60:1:23:12:150. The mixed gel is allowed to stand at 70°C for 5 hours and then subjected to crystallization treatment; the crystallization treatment adopts a steam-assisted crystallization method, the crystallization treatment temperature is 170°C, and the crystallization time is 24 hours.

[0067] B. The crystallized product is first calcined at a temperature of 340°C for 6 hours. Then, an aluminum ion source is used to dope the crystallized product by ion implantation. The aluminum ion source used for ion implantation is trimethylaluminum. The flow rate of the aluminum ion source is 80 sccm, the voltage is 30 kV, and the pressure is 1×10 -3 Pa~3×10 -3 Pa, the treatment time is 0.5h. Then the crystallized product is calcined for the second time, the temperature of the second calcination is 650°C, the time of the second calcination is 12h, and the Cu-SSZ-13 molecular sieve is obtained.

[0068] C. Crush the Cu-SSZ-13 molecular sieve, add it into an ethanol aqueous solution and stir it, then add polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine, the ethanol content of the ethanol aqueous solution is 60wt%, and the mass ratio of Cu-SSZ-13 molecular sieve, ethanol aqueous solution, polyvinyl pyrrolidone, Ce(NO3)3·6H2O and hexamethylenetetramine is 1:1200:10:1:2. After stirring for 2h, reflux at 60°C for 2h, filter, wash, and dry, and then calcine at a temperature of 500°C for 12h to obtain a cerium-modified Cu-SSZ-13 molecular sieve (the molecular sieve prepared in this embodiment is recorded as Cu-SSZ-13@CeO2-5).

[0069] The molecular sieves prepared in the above examples and comparative examples were used to carry out performance tests.

[0070] The ammonia oxidation performance of each test sample was tested in the temperature range of 150℃~400℃, and the gas composition was N2, O2, and NH3. The NH3 concentration was 50ppm, O2 was 4%, and N2 was used as the balance gas to pass into the reactor. The results are shown in Figure 1 . Within the scope of investigation, the ammonia oxidation efficiency of the catalyst remained above 65%, and increased with the increase of temperature. When the temperature reached 300°C, the ammonia removal rate could basically reach 100%, which effectively reflects the promoting effect of temperature increase on ammonia oxidation efficiency. In the temperature range of 200°C to 400°C, the ammonia oxidation activity of Cu-SSZ-13 modified with cerium is higher than that of Cu-SSZ-13, indicating that cerium modification is beneficial to the improvement of ammonia oxidation activity. Among them, the ammonia oxidation efficiency of the Cu-SSZ-13@CeO2-2 catalyst is the best, reaching 100% at 200°C.

[0071] See also Figure 2 The catalyst has roughly the same change trend in the temperature range of 150℃~400℃. The nitrogen selectivity is the highest at 150℃, which is above 97%. x The nitrogen selectivity of each catalyst decreases with increasing temperature, and the higher the temperature, the faster the decrease rate. Compared with Cu-SSZ-13, the nitrogen selectivity of the cerium-modified Cu-SSZ-13 catalyst decreases slightly, indicating that cerium modification slightly promotes the production of by-products. At low temperatures, the nitrogen selectivity of each catalyst is high and will not lead to the generation of a large number of by-products.

[0072] NO was introduced under the above conditions to explore the effect of NO at different temperatures. x The results of the effects of various catalysts on the ammonia oxidation performance are shown in Figure 3. After adding NO, the ammonia oxidation efficiency of Cu-SSZ-13 and Cu-SSZ-13 modified by cerium was improved, and basically reached more than 80% within the scope of investigation. With the increase of temperature, the ammonia oxidation performance of each catalyst also gradually increased, and the temperature required for complete removal was lower than that when no NO was added. The ammonia oxidation efficiency of Cu-SSZ-13 modified by cerium was still higher than that of Cu-SSZ-13, and Cu-SSZ-13@CeO2-2 had the best catalytic effect, which was higher than 92.6% at 150°C.

[0073] See also Figure 4 When NO was added, the change trend of nitrogen selectivity of each catalyst was the same as that without NO, and they all gradually decreased with the increase of temperature, and could still be maintained above 85% at 400℃.

[0074] Figure 5 The denitrification performance of the catalyst was demonstrated. As the temperature continued to rise, the denitrification efficiency of each catalyst gradually increased and then decreased. The denitrification efficiency of the Cu-SSZ-13 catalyst remained above 80% at 200℃~350℃, while the cerium-modified Cu-SSZ-13 had a higher denitrification activity below 250℃ and was lower above 300℃, which may be due to the significant promotion of the reaction of NH3 and O2 at high temperature, resulting in insufficient NO reducing agent. The denitrification efficiency of Cu-SSZ-13@CeO2 reached the highest at 250℃. At this temperature, the denitrification effect of Cu-SSZ-13@CeO2-2 catalyst was the best, with an efficiency of 87.7%.

[0075] Mercury oxidation experiment: the inlet Hg 0 The concentration was controlled at 72 μg / m 3 , record the data after the data is stable for 30 minutes. Figure 6 As shown in the figure, as the temperature increases, the mercury oxidation activity of each catalyst gradually increases at 150℃~200℃, and gradually decreases above 200℃. This may be because too high a temperature is not conducive to the oxidation of Hg 0 Compared with Cu-SSZ-13, the mercury oxidation efficiency of Cu-SSZ-13 modified by cerium is improved, and it is maintained above 97% at 200℃~300℃.

[0076] Based on the flue gas conditions of the mercury oxidation performance test, 50 ppm of ammonia was introduced to explore the mercury oxidation performance of each catalyst in the presence of ammonia. Figure 7As shown in the figure, after the addition of ammonia, the mercury oxidation efficiency of each catalyst at 150℃~200℃ did not change significantly compared with the efficiency without ammonia. After 200℃, as the temperature continued to rise, the mercury oxidation performance of each catalyst began to decline sharply, and the mercury oxidation efficiency was less than 25% at 400℃. This result shows that the presence of ammonia has a certain inhibitory effect on the mercury oxidation reaction, which may be due to the fact that NH3 and Hg 0 Competitive adsorption of adsorption sites and competitive consumption of active oxygen. Since the ammonia oxidation reaction is promoted at high temperatures and the active oxygen on the catalyst surface is consumed, the inhibitory effect is more obvious at high temperatures. In contrast, low temperatures are more conducive to the oxidation and removal of mercury in ammonia-containing flue gas.

[0077] Based on the flue gas conditions of the ammonia oxidation performance test, mercury vapor was introduced to explore the effect of mercury on the ammonia oxidation performance of each catalyst. Figure 8 As shown in the figure, in the presence of mercury, the ammonia oxidation performance of each catalyst is not much different from the previous one, and gradually increases with the increase of temperature, reaching 100% after 300°C. This result shows that the lower concentration of Hg in the flue gas 0 It will not have a significant effect on the ammonia oxidation reaction.

[0078] Next, the Cu-SSZ-13@CeO2-2 with better ammonia oxidation performance and the Cu-SSZ-13 molecular sieve without cerium modification were selected to test the anti-sulfur performance at 250°C. When SO2 was not introduced, the oxidation efficiency of the Cu-SSZ-13@CeO2-2 catalyst could reach 100%, and the ammonia oxidation efficiency of the Cu-SSZ-13 molecular sieve was 88.6%. After SO2 was introduced, the ammonia oxidation efficiency of the catalyst was inhibited, and the ammonia oxidation efficiency of the Cu-SSZ-13 molecular sieve dropped to 82.6%, and the ammonia oxidation efficiency of the Cu-SSZ-13@CeO2-2 catalyst dropped to 89.5%. Both of them recovered slightly after cutting off SO2. The results show that SO2 has a certain irreversible inhibitory effect on the ammonia oxidation reaction of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 catalysts. The reason may be that SO2 reacts with the active species on the catalyst surface to form sulfate or sulfite, blocking the oxidation reaction path of NH3. In contrast, under 500 ppm SO2, the ammonia oxidation efficiency of the Cu-SSZ-13@CeO2-2 catalyst is still close to 90%, indicating that cerium modification is beneficial to the efficient oxidation of ammonia in sulfur-containing flue gas.

[0079] like Fig.10 As shown, the nitrogen selectivity of the two catalysts was slightly improved by adding SO2, and there was no obvious change after cutting off SO2, indicating that SO2 has little effect on nitrogen selectivity.

[0080] Subsequently, the effects of SO2 on the ammonia oxidation and denitrification performance of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 catalysts in the presence of NO were also investigated. Fig.11 When NO is present, the ammonia oxidation efficiency of the two catalysts is improved, and the sulfur resistance is also good. After adding SO2, the ammonia oxidation efficiency of the two catalysts decreases slightly, maintaining 90.4% and 90.7% ammonia oxidation efficiency respectively. After cutting off SO2, the ammonia oxidation efficiency is slightly improved compared with when it is introduced.

[0081] As shown in Figure 12, after adding SO2, the denitration efficiency of the two catalysts dropped sharply, only 18.4% and 35.2%, and rose to 22.7% and 41.4% after cutting off SO2. This shows that the presence of SO2 has a significant inhibitory effect on the denitration efficiency of the catalyst. In addition, after the introduction of SO2, the nitrogen selectivity of the catalyst increased slightly, similar to the case without the introduction of NO. After cutting off SO2, the nitrogen selectivity did not change compared to when SO2 was added. Fig.13 shown.

[0082] Next, the effect of SO2 on the mercury oxidation performance of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 at 250°C was tested. Fig.14 The data showed that the mercury oxidation efficiency of the two catalysts decreased slightly after adding SO2, to 89.3% and 96.4% respectively. After cutting off SO2, the mercury oxidation efficiency of the two catalysts basically returned to the level before adding SO2, indicating that the inhibitory effect of SO2 on mercury oxidation was not obvious.

[0083] Characterization analysis of Cu-SSZ-13 and Cu-SSZ-13-CeO2-2.

[0084] The microstructure of Cu-SSZ-13@CeO2-2 was observed by HR-TEM. Fig.15 As shown, the catalyst showed a typical rhombohedral structure of molecular sieves, and a large number of CeO2 crystals with a diameter of 4 to 8 nm appeared on the surface of the molecular sieve, exposing the CeO2 (111) crystal plane (lattice spacing 0.31 nm). Line scan and surface scan results showed that the catalyst was rich in a large amount of Si and O elements and a small amount of Al, Cu, and Ce elements, among which Si, O, Al, and Cu were evenly distributed in the catalyst, while the Ce element was more densely distributed at the edge of the catalyst particles, indicating that Ce was mainly coated on the surface of the catalyst Cu-SSZ-13 molecular sieve in the form of small CeO2 clusters.

[0085] The N2 adsorption-desorption curve and pore size distribution of the catalyst are shown in Fig.16 , 17. Both Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 are type I isotherms with H4-type hysteresis loops, indicating that they are hierarchical porous systems including micropores and mesopores. The data in Table 1 show that the specific surface area of ​​the catalyst did not decrease after CeO2 coating, but increased, and the pore volume and pore size increased. This shows that the stacking of small CeO2 grains on the surface of Cu-SSZ-13 will not block the pores, and the preparation process produces more porous structures, which may be beneficial to the adsorption and diffusion of reactant molecules.

[0086] Table 1

[0087] catalyst <![CDATA[Specific surface area, m 2 / g]]> <![CDATA[Pore volume, cm 3 / g]]> Average pore size, nm Cu-SSZ-13 462.58 0.06 10.43 <![CDATA[Cu-SSZ-13@CeO2-2]]> 552.98 0.08 13.55

[0088] The XRD patterns of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 are shown in Fig.18 As shown, both exhibit typical diffraction peaks attributed to CHA structure and CuO. Compared with the Cu-SSZ-13 catalyst, the XRD peak intensity corresponding to the CHA and CuO structures of the Cu-SSZ-13@CeO2-2 catalyst is significantly reduced, which should be due to the wrapping of Cu-SSZ13 by the CeO2 shell, which is consistent with the HR-TEM observation results. In addition, Cu-SSZ-13@CeO2-2 does not show obvious crystal peaks of CeO2, which may be due to the fact that the grain size of CeO2 on its surface is lower than the XRD detection limit.

[0089] XPS was used to analyze the valence distribution of O, Cu, and Ce in Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 catalysts. Figure 19-21 The data are summarized in Table 2. It can be found that the O in the Cu-SSZ-13 catalyst is in the form of chemically adsorbed oxygen (O α ) exists in the form of, and after coating with CeO2, lattice oxygen (O β ), combined with HR-TEM results, it is believed that it mainly comes from the CeO2 crystals coated on the surface. In addition, the valence state of Cu in the catalyst changes after coating with CeO2. 2+ The ratio decreased, Cu + The increase in the ratio indicates that CeO2 on the surface interacts with copper oxide to a certain extent, which promotes the transformation of Cu to a low-valent state. 4+ The proportion is much higher than Ce 3+ , which also proves that Ce in the catalyst mainly exists in the form of CeO2.

[0090] Table 2

[0091]

[0092] In order to reveal the mechanism of the effect of cerium modification on the ammoxidation of Cu-SSZ-13, in situ infrared spectroscopy was used to identify the NH3 species adsorbed on the surface of Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 and their reaction with O2. Fig. 22 As shown in the figure, after 30 min of NH3 pretreatment, the two catalysts showed -1 、1270cm -1 and 1190cm -1 The Lewis acidic site adsorbed NH3 species appeared, 1743 cm -1 and 1434cm -1 Appeared NH4 adsorbed on acidic sites + It can be seen that Cu-SSZ-13 has a larger number of Lewis acid sites, while Cu-SSZ-13@CeO2-2 has more Acidic position, and at 1340cm -1 A small amount of intermediate product -NH2 of ammonia oxidation appeared, indicating that the coated cerium species provided a new Acidic site, which is conducive to the activation of NH3. Fig.23 It shows that after the introduction of O2, the content of NH3 adsorbed on the Lewis acidic site of Cu-SSZ-13 gradually decreases. Acidic NH4 + There was no significant decrease in species, including 1434cm -1 The peak of NH4 adsorbed on acidic sites + Species are not easily oxidized. Fig.24 It is shown that the Cu-SSZ-13@CeO2-2 catalyst is adsorbed on Lewis and The ammonia species in the acidic site decreased significantly with the introduction of O2, that is, the The acidic sites also have ammonia oxidation activity, which may be one of the reasons for the increase in the ammonia oxidation efficiency of the catalyst after cerium modification.

[0093] Fig.25 The temperature-programmed desorption curves of mercury for Cu-SSZ-13 and Cu-SSZ-13@CeO2-2 catalysts are shown in Figure 2. The data show that Cu-SSZ-13 only has a broad mercury desorption peak at 592.7°C, which corresponds to the decomposition of HgO adsorbed on its surface. 0 After being oxidized by the catalyst, it can stay on the catalyst surface in the form of HgO. The Cu-SSZ-13@CeO2-2 catalyst showed two new peaks at 140.2℃ and 166.1℃, which were identified as physically adsorbed Hg 0The results show that cerium modification increases two types of mercury adsorption sites, which may come from the newly added cerium species or the interaction between cerium and copper species, which is beneficial to Hg 0 In addition, Cu-SSZ-13@CeO2-2 did not show an obvious desorption peak above 200 °C, which may be due to the Hg 0 The HgO generated by oxidation will not stay on the catalyst surface, but can be completely desorbed and enter the flue gas.

[0094] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing cerium-modified Cu-SSZ-13 molecular sieve, Features The following steps are involved: A. Sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, and benzyltrimethylamine were mixed with water to prepare a mixed gel, which was allowed to stand at 70° C. for 5 hours and then subjected to crystallization treatment; B. calcining the crystallized product for the first time, then doping the crystallized product by ion implantation using an aluminum ion source, and then calcining the crystallized product for the second time to obtain a Cu-SSZ-13 molecular sieve; C. Crush the Cu-SSZ-13 molecular sieve, add it into ethanol aqueous solution and stir it, then add polyvinyl pyrrolidone, Ce(NO 3 ) 3 6H 2 O and hexamethylenetetramine, stirred for 2 h, refluxed at 60 ° C for 2 h, filtered, washed, dried and then calcined to obtain cerium-modified Cu-SSZ-13 molecular sieve.

2. The method for preparing the cerium-modified Cu-SSZ-13 molecular sieve according to claim 1, Features: In step A, the molar ratio of sodium hydroxide, sodium silicate, aluminum sulfate, copper sulfate, benzyltrimethylamine and water is 1:60:1:23:12:

150.

3. The method for preparing the cerium-modified Cu-SSZ-13 molecular sieve according to claim 2, Features: In step A, the crystallization treatment adopts a steam-assisted crystallization method, the crystallization treatment temperature is 170° C., and the crystallization time is 24 hours.

4. The method for preparing the cerium-modified Cu-SSZ-13 molecular sieve according to claim 3, Features: In step B, the temperature of the first calcination is 340° C., and the time of the first calcination is 6 hours; the temperature of the second calcination is 650° C., and the time of the second calcination is 12 hours.

5. The method for preparing the cerium-modified Cu-SSZ-13 molecular sieve according to claim 4, Features: In step B, the aluminum ion source used for ion implantation is trimethylaluminum, the flow rate of the aluminum ion source is 80 sccm, the voltage is 30 kV, and the pressure is 1×10 -3 Pa~3×10 -3 Pa, processing time is 0.5h.

6. The method for preparing the cerium-modified Cu-SSZ-13 molecular sieve according to claim 4, Features: In step C, the ethanol content of the ethanol aqueous solution is 60wt%, Cu-SSZ-13 molecular sieve, ethanol aqueous solution, polyvinyl pyrrolidone, Ce(NO 3 ) 3 6H 2 The mass ratio of O and hexamethylenetetramine is 1:1200:10:3:

2.

7. The method for preparing the cerium-modified Cu-SSZ-13 molecular sieve according to claim 6, Features: In step C, the calcination temperature is 500° C. and the calcination time is 12 h.

8. A cerium-modified Cu-SSZ-13 molecular sieve, Features: The cerium-modified Cu-SSZ-13 molecular sieve is prepared by the preparation method of any one of claims 1 to 7.

Citation Information

Patent Citations

  • Preparation method of Ce modified Cu-Fe-SSZ-13 molecular sieve

    CN112844463A

  • SCR catalyst and preparation method

    WO2020249105A1

Cited By

  • Core-shell type molecular sieve catalyst as well as preparation method and application thereof

    CN120394076A