Process for preparing ferric nitrate by leaching iron resources and application of process

By combining the leaching agent with concentrated nitric acid, the problem of iron oxide not reacting with nitric acid was solved, enabling the efficient preparation of ferric nitrate, reducing the raw material cost of lithium iron phosphate, and achieving efficient recovery and recycling of iron resources.

CN118929767APending Publication Date: 2024-11-12QUJING DYNANONIC CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411017179.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In existing technologies, iron oxide, especially iron oxide red, basically does not react with nitric acid, which limits its application as an iron source material for the liquid-phase preparation of lithium iron phosphate.

Method used

The iron oxide source is mixed, ground, and heated to leach using a combination of leaching agent and concentrated nitric acid. This provides a reduction potential, increases the leaching rate of iron ions, and forms ferric nitrate.

Benefits of technology

It significantly improved the leaching rate of iron oxide source, and the concentration and purity of ferric nitrate in the leachate were high, which reduced the raw material cost for preparing lithium iron phosphate and realized the efficient recovery and recycling of iron resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929767A_ABST
    Figure CN118929767A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of iron resource utilization, and particularly relates to a technology for preparing ferric nitrate through iron resource leaching and application of the technology. Comprising the following steps: mixing and grinding an iron oxide source and a leaching agent to obtain a mixed material; the leaching agent provides reduction potential; the mixed material and concentrated nitric acid are mixed and then subjected to a leaching reaction under the heating condition, leaching liquid and leaching residues are obtained through separation, and the leaching liquid comprises ferric nitrate. According to the technology, the leaching agent is combined with concentrated nitric acid to conduct the leaching reaction on the iron oxide source, the leaching agent can reduce the reduction potential and the reaction activation energy, the reaction of nitric acid and the iron oxide source is accelerated, and the leaching rate of the iron oxide source in nitric acid is remarkably increased. The iron resource extraction and recovery efficiency is high, the iron resource can be directly used as an iron source for preparing the phosphate iron salt positive electrode material by the liquid phase method, and the cost of the iron source raw material for preparing the phosphate iron salt positive electrode material by the liquid phase method is reduced. And moreover, leaching residues can be recycled, and the method is economical, environmentally friendly and suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of iron resource utilization, and in particular relates to a process for preparing ferric nitrate by leaching iron resources and its application. Background Art

[0002] Lithium iron phosphate (LiFePO 4 , abbreviated as LFP) is a positive electrode material for lithium-ion batteries. With its advantages of high safety, high cycle life, low cost and wide source of raw materials, it has become the first choice for new energy vehicles and energy storage scenarios. In the face of new opportunities, the development of new process technologies for lithium iron phosphate, especially reducing raw material costs and simplifying process flows, is particularly important for improving the economy and product quality of lithium iron phosphate. From the perspective of production process, lithium iron phosphate is mainly divided into solid phase method and liquid phase method. In the solid phase method, the iron source, phosphorus source and lithium source are uniformly ground by mechanical grinding and then calcined at high temperature to form carbon coating to prepare lithium iron phosphate; in the liquid phase method, the raw materials are mixed in a liquid, and a gel precursor is prepared by self-heating and then sintered to prepare lithium iron phosphate. According to the iron source used in different production processes, it can be further divided into four routes: solid phase method + iron phosphate, solid phase method + ferrous oxalate, liquid phase method + ferric nitrate, and liquid / solid phase method + iron red.

[0003] Although there are differences in the cost reduction paths of different process routes, the fundamental goal is to reduce the cost of raw materials. The cost of lithium iron phosphate raw materials depends on the upstream lithium source, phosphorus source, iron source, etc. The process route of lithium iron manganese phosphate is the same as that of lithium iron. Among them, the liquid phase method + ferric nitrate process has a wide range of raw material sources. Iron blocks and nitric acid can be purchased to make ferric nitrate to reduce the synthesis cost and alleviate the bottleneck of precursor supply. As a source of iron, iron red has a wide source, low cost, non-toxic and environmentally friendly materials, and low cost. Iron oxide connects multiple cost reduction routes. Battery-grade iron oxide can use pyrite / hematite as raw materials. Domestic pyrite resources are abundant and are one of the important sources of iron oxide. Battery-grade iron oxide can also be obtained by purifying and treating the iron sheets produced as a by-product of pickling in steel rolling mills to obtain battery-grade iron oxide.

[0004] The iron oxide + nitric acid route can significantly save production and environmental protection costs. However, iron oxide, especially γ-Fe 2 O 3 The red iron oxide in the liquid phase basically does not react with nitric acid, which greatly limits the use of red iron oxide and other iron oxides to prepare iron nitrate as an iron source material for preparing lithium iron phosphate by the liquid phase method. Summary of the invention

[0005] The purpose of the present application is to provide a process for preparing ferric nitrate by leaching iron resources and its application, aiming to solve to a certain extent the problem that existing iron oxide resources such as red iron oxide basically do not react with nitric acid, which limits the use of iron oxide resources such as red iron oxide to prepare ferric nitrate for the liquid phase preparation of lithium iron phosphate.

[0006] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0007] In a first aspect, the present application provides a process for preparing ferric nitrate by leaching iron resources, comprising the following steps:

[0008] The iron oxide source and the leaching agent are mixed and ground to obtain a mixed material; the leaching agent provides a reducing potential;

[0009] After the mixed material is mixed with concentrated nitric acid, a leaching reaction is carried out under heating conditions to separate and obtain a leaching solution and a leaching residue, wherein the leaching solution includes ferric nitrate.

[0010] In some possible implementations, the purity of the ferric nitrate in the leaching solution is not less than 99.9%.

[0011] In some possible implementations, the leaching solution is directly used as an iron source for preparing an iron phosphate-based positive electrode material by a liquid phase method.

[0012] In some possible implementations, the iron oxide source includes at least one of red iron, ferroferric oxide, hematite, and magnetite.

[0013] In some possible implementations, the leaching agent includes at least one of a reducing agent and a catalyst.

[0014] In some possible implementations, the reducing agent includes at least one of carbon powder, white phosphorus, sucrose, glucose, acetic acid, formic acid, benzoic acid, and starch.

[0015] In some possible implementations, the catalyst includes TiO 2 、MnO 2 , Pt, Pd, Rh.

[0016] In some possible implementations, the mass ratio of the iron oxide source to the leaching agent is 100:(1-100).

[0017] In some possible implementations, the mixed grinding conditions include: ball milling for 1 h to 10 h at a rotation speed of 600 rpm to 1500 rpm.

[0018] In some possible implementations, the particle size of the particles in the mixed material is 200-1000 mesh.

[0019] In some possible implementations, the mass fraction of the concentrated nitric acid is 45% to 100%.

[0020] In some possible implementations, the mass ratio of the mixed material to the concentrated nitric acid is 1:(1-20).

[0021] In some possible implementations, the leaching reaction conditions include: leaching for 6 h to 24 h at a temperature of 90° C. to 150° C. and a stirring rate of 300 rpm to 800 rpm.

[0022] In some possible implementations, the method further includes the steps of: recycling the leaching residue to obtain an unreacted leaching agent; and recycling the unreacted leaching agent to a process for leaching iron resources to prepare ferric nitrate.

[0023] In a second aspect, an embodiment of the present application provides an application of the process for preparing ferric nitrate by leaching iron resources as described above, and applies the process for preparing ferric nitrate by leaching iron resources to the field of lithium-ion batteries.

[0024] The process for preparing ferric nitrate by leaching iron resources provided in the first aspect of the present application adopts a leaching agent, combined with concentrated nitric acid, to carry out a leaching reaction on an iron oxide source, wherein the leaching agent can provide a reduction potential for the iron oxide source in the reaction, thereby reducing the reduction potential of the iron oxide source, so that the iron ions in the iron oxide source can be efficiently and quickly leached to form ferric nitrate, and the leaching rate of the iron oxide source in nitric acid is significantly improved. The process route is short, the operation is simple, and there are few by-products. The leached ferric nitrate is concentrated in the leachate, with high concentration and purity, and high efficiency of iron resource extraction and recovery. It can be directly used as an iron source for preparing ferric phosphate-based positive electrode materials such as lithium iron phosphate and lithium manganese iron phosphate by liquid phase method, which reduces the synthesis cost of ferric nitrate and alleviates the raw material supply cost for preparing ferric phosphate-based positive electrode materials. The leached slag is mainly composed of unreacted iron oxide sources and leaching agents, which can be recycled and reused again, which is not only economical and environmentally friendly, but also forms an industrial closed loop, suitable for industrial applications.

[0025] The ferric nitrate prepared by the process of preparing ferric nitrate by leaching the above-mentioned iron resources in the present application can be directly used as an iron source in the field of lithium-ion batteries, and is particularly suitable for preparing an iron source for ferric phosphate-based positive electrode materials by a liquid phase method. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0027] Figure 1 It is a schematic flow chart of a process for preparing ferric nitrate by leaching iron resources provided in an embodiment of the present application;

[0028] Figure 2 It is a schematic flow chart of the iron red leaching process provided in Example 1 of the present application. DETAILED DESCRIPTION

[0029] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0030] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0031] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0032] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0033] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0034] The weight of the relevant components mentioned in the embodiments of the present specification can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components in the embodiments of the present specification is proportionally enlarged or reduced, it is within the scope disclosed in the embodiments of the present specification. Specifically, the mass described in the embodiments of the present specification can be μg, mg, g, kg and other mass units known in the chemical industry.

[0035] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0036] In a first aspect, the present invention provides a process for preparing ferric nitrate by leaching iron resources, as shown in the attached Figure 1 As shown, the following steps are included:

[0037] S10. The iron oxide source and the leaching agent are mixed and ground to obtain a mixed material; the leaching agent provides a reducing potential;

[0038] S20. After mixing the mixed material with concentrated nitric acid, a leaching reaction is carried out under heating conditions to separate a leachate and a leach residue, wherein the leachate includes ferric nitrate.

[0039] The process for preparing ferric nitrate by leaching iron resources provided in the first aspect of the embodiment of the present application adopts a leaching agent, combined with concentrated nitric acid, to carry out a leaching reaction on an iron oxide source, wherein the leaching agent can provide a reduction potential for the iron oxide source in the reaction, thereby reducing the activation energy of the reaction, reducing the reduction potential of the reaction, so that the iron ions in the iron oxide source can be efficiently and quickly leached to form ferric nitrate, and significantly improve the leaching rate of the iron oxide source in nitric acid. The process route is short, the operation is simple, and there are few by-products. The leached ferric nitrate is concentrated in the leachate, with high concentration and purity, and high efficiency of iron resource extraction and recovery. It can be directly used as an iron source for preparing ferric phosphate-based positive electrode materials such as lithium iron phosphate and lithium manganese iron phosphate by liquid phase method, reducing the cost of ferric nitrate synthesis and alleviating the cost of raw material supply for preparing ferric phosphate-based positive electrode materials. The leached slag is mainly composed of unreacted iron oxide sources and leaching agents, which can be recycled and reused again, which is not only economical and environmentally friendly, but also forms an industrial closed loop, suitable for industrial applications.

[0040] In the above step S10:

[0041] In some possible implementations, the iron oxide source includes at least one of iron oxide red, ferroferric oxide, hematite, and magnetite. 2 O 3 The iron oxide phase basically does not react with nitric acid. The chemical formula of ferroferric oxide is Fe 3 O 4 , which is a black crystal with magnetic properties, can be roughly regarded as a compound composed of ferrous oxide and ferric oxide (FeO·Fe 2 O 3), natural ferroferric oxide is insoluble in acid solution and is easily oxidized to iron oxide (Fe 2 O 3 ). The chemical composition of hematite is Fe 2 O 3 , an oxide mineral of the hexagonal system. Magnetite refers to the ore of the oxide mineral magnetite, the main component of which is Fe 3 O 4 These iron sources are rich in Fe 2 O 3 The iron ions in the iron oxide source can be leached quickly and efficiently by combining a leaching agent with concentrated nitric acid to produce ferric nitrate.

[0042] In some possible implementations, the iron oxide source includes red iron oxide. In this case, red iron oxide can better reduce costs, the material is non-toxic and environmentally friendly, and the iron oxide connects multiple cost reduction routes.

[0043] In some possible implementations, the leaching agent includes at least one of a reducing agent and a catalyst. In this case, both the reducing agent and the catalyst can provide a reduction potential for the leaching of iron ions, so that the iron ions in the iron oxide source can be efficiently and quickly leached to form iron nitrate, significantly improving the leaching rate of the iron oxide source in nitric acid.

[0044] In some possible implementations, the reducing agent includes at least one of carbon powder, white phosphorus, sucrose, glucose, acetic acid, formic acid, benzoic acid, and starch. These reducing agents used in the embodiments of the present application can provide a reduction potential for the iron oxide source, reduce the iron oxide source, and obtain the target product of iron nitrate.

[0045] In some embodiments, the reducing agent includes carbon powder, and the steps of reducing and leaching red iron oxide include the following:

[0046] First step reaction: C + 6HNO 3 +Fe 2 O 3 =2Fe(NO 3 ) 2 +3H 2 O+CO 2 ↑+2NO 2 ↑;

[0047] The second step reaction: 3Fe(NO 3 ) 2 +4HNO 3 =3Fe(NO 3 ) 3 +NO↑+2H 2 O;

[0048] Overall reaction: 3C + 26HNO 3 +3Fe2 O 3 =6Fe(NO 3 ) 3 +13H 2 O+3CO 2 ↑+6NO 2 ↑+2NO↑.

[0049] In some embodiments, the reducing agent includes carbon powder, and the step of reducing and leaching ferroferric oxide includes: Fe 3 O 4 +11HNO 3 +C=3Fe(NO 3 ) 3 +CO 2 +5H 2 O+NO 2 +NO.

[0050] In some possible implementations, the catalyst includes TiO 2 、MnO 2 At least one of Pt, Pd, and Rh. The catalysts used in the embodiments of the present application can provide a reduction potential for the iron oxide source, reduce the reaction activation energy, accelerate the reaction between nitric acid and the iron oxide source, and generate the target product, iron nitrate.

[0051] In some embodiments, the catalyst comprises TiO 2 The steps of catalytic leaching of red iron oxide include the following:

[0052] Fe 2 O 3 +6HNO 3 =2Fe(NO 3 ) 3 +3H 2 O.

[0053] In some embodiments, the catalyst comprises MnO 2 The steps of catalytic leaching of red iron oxide include the following:

[0054] First step reaction: 2MnO 2 +6HNO 3 +Fe 2 O 3 =2MnO 3 +2Fe(NO 3 ) 2 +2NO 2 ↑+3H 2 O;

[0055] Second step reaction: 2MnO 3 =2MnO 2 +O 2↑.

[0056] In some possible implementations, the leaching agent includes a reducing agent and a catalyst. In this case, the leaching agent contains both a reducing agent and a catalyst, which can better provide a reduction potential for the leaching of the iron oxide source, reduce the reaction activation energy, and efficiently and quickly obtain the iron nitrate leachate. In some embodiments, in the leaching agent, the mass ratio of the reducing agent to the catalyst can be 1:1, 1:2, 1:3, 0.5:1, 0.8:1, 0.3:1, etc.

[0057] In some possible implementations, the mass ratio of the iron oxide source to the leaching agent is 100:(1-100). In this case, it is beneficial to improve the leaching efficiency of the iron oxide source and to control the reaction rate and cost. Exemplarily, the mass ratio of the iron oxide source to the leaching agent can be 100:1, 100:10, 100:20, 100:30, 100:40, 100:50, 100:60, 100:70, 100:80, 100:90, 100:100, etc., typical but non-limiting arbitrary point values ​​or interval values ​​between any two point values.

[0058] In some possible implementations, the conditions for mixed grinding include: ball milling for 1h to 10h at a rotation speed of 600rpm to 1500rpm. Under such conditions, by fully mixed grinding, the particle size of the iron oxide source and the leaching agent can be refined, and the contact performance of the iron oxide source and the leaching agent can be improved, so that the two are fully in contact, which is convenient for subsequent uniform and stable leaching. Exemplarily, the rotation speed of mixed grinding can be 600rpm, 700rpm, 800rpm, 900rpm, 1000rpm, 1100rpm, 1200rpm, 1400rpm, 1500rpm, etc., typical but non-limiting arbitrary point values ​​or interval values ​​between any two point values, and the grinding time can be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, etc., typical but non-limiting arbitrary point values ​​or interval values ​​between any two point values.

[0059] In some possible implementations, the particle size of the particles in the mixed material is 200 to 1000 mesh. In this case, the iron oxide source and the leaching agent in the mixed material both have a smaller particle size, which is conducive to uniform mixing and to improving the subsequent leaching efficiency. Exemplarily, the particle size of the particles in the mixed material can be 200 mesh, 300 mesh, 500 mesh, 600 mesh, 800 mesh, 1000 mesh, etc., typical but non-limiting arbitrary point values ​​or interval values ​​between any two point values.

[0060] In the above step S20:

[0061] In some possible implementations, the mass fraction of concentrated nitric acid is 45% to 100%. In this case, concentrated nitric acid can react with the mixed material more efficiently and quickly, increase the reduction charge, increase the leaching reaction rate, and increase the leaching recovery rate of iron nitrate. Exemplarily, the mass fraction of concentrated nitric acid can be 45%, 50%, 60%, 70%, 80%, 90%, 100%, etc., typical but non-limiting arbitrary point values ​​or interval values ​​between any two point values.

[0062] In some possible implementations, the mass ratio of the mixture to concentrated nitric acid is 1:(1-20). In this ratio, it is beneficial for concentrated nitric acid to quickly and efficiently leach ferric nitrate. Exemplarily, the mass ratio of the mixture to concentrated nitric acid can be 1:1, 1:3, 1:5, 1:8, 1:10, 1:12, 1:15, 1:18, 1:20, etc., typical but non-limiting arbitrary point values ​​or interval values ​​between any two point values.

[0063] In some possible implementations, the leaching reaction conditions include: leaching for 6h to 24h at a temperature of 90°C to 150°C and a stirring rate of 300rpm to 800rpm. Under such reaction conditions, it is beneficial to improve the efficiency of the leaching reaction and ensure the safety and controllability of the reaction. Exemplarily, the temperature conditions of the leaching reaction can be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc., typical but non-limiting arbitrary point values ​​or interval values ​​between any two point values, the speed can be 300rpm, 400rpm, 500rpm, 600rpm, 700rpm, 800rpm, etc., typical but non-limiting arbitrary point values ​​or interval values ​​between any two point values, and the duration can be 6h, 8h, 10h, 12h, 14h, 15h, 18h, 20h, 22h, 24h, etc., typical but non-limiting arbitrary point values ​​or interval values ​​between any two point values.

[0064] In some embodiments, the process of leaching iron resources to prepare ferric nitrate in the present application has a leaching rate of more than 95% for iron in iron oxide sources, and has a high iron leaching recovery efficiency. It can be directly used as an iron source for preparing lithium iron phosphate, lithium manganese iron phosphate and other iron phosphate-based positive electrode materials by the liquid phase method, thereby reducing the cost of iron source raw materials for preparing iron phosphate-based positive electrode materials by the liquid phase method.

[0065] In some possible implementations, the leaching residue is recycled to obtain an incompletely reacted leaching agent; the incompletely reacted leaching agent is cyclically applied to the process of leaching iron resources to prepare ferric nitrate. The leaching residue in the embodiment of the present application mainly contains an incompletely reacted iron oxide source and a leaching agent, and the leaching liquid is ferric nitrate. By recycling the iron oxide source and the leaching agent in the leaching residue, the recovered iron oxide source and the leaching agent can be reused, and after calculating and replenishing the loss, they can be cyclically put into the process of leaching iron resources to prepare ferric nitrate, thereby improving the resource utilization rate.

[0066] In some embodiments, the leaching agent is TiO 2 When the leaching agent is MnO, it is not consumed in the reaction and does not need to be replenished. 2 Due to the skewing reaction during the reaction, 5% will be dissolved (calculated by ICP inductively coupled plasma test of leached slag phase), so 5% new MnO needs to be added each time. 2 .

[0067] In some embodiments, the leaching agent is a reducing agent, which will be consumed in the reaction and needs to be supplemented with a new reducing agent. The consumption of different reducing agents each time is also different. For example, when the leaching agent is carbon powder, 4% is consumed each time. After the leaching residue is digested with hydrochloric acid, the remainder is the recovered carbon powder, which is used again in the process of leaching iron resources to prepare ferric nitrate, and 4% of new carbon powder needs to be supplemented.

[0068] In some possible implementations, the purity of the ferric nitrate in the leachate is not less than 99.9%; the embodiment of the present application not only has a high efficiency in iron resource extraction and recovery, but also has a high concentration and purity of ferric nitrate in the leachate, and can be directly used as an iron resource.

[0069] In some possible implementations, the leachate is directly used as an iron source in the preparation of ferric phosphate-based positive electrode materials by the liquid phase method, which can significantly reduce the cost of iron source raw materials for the preparation of ferric phosphate-based positive electrode materials by the liquid phase method. Among them, ferric phosphate-based positive electrode materials include but are not limited to lithium iron phosphate, lithium iron manganese phosphate, etc.

[0070] In a second aspect, an embodiment of the present application provides an application of the process for preparing ferric nitrate by leaching iron resources as described above, and applies the process for preparing ferric nitrate by leaching iron resources to the field of lithium-ion batteries.

[0071] The ferric nitrate prepared by the process of preparing ferric nitrate by leaching iron resources in the embodiment of the present application can be directly used as an iron source in the field of lithium-ion batteries, and is particularly suitable for preparing an iron source for ferric phosphate-based positive electrode materials by a liquid phase method.

[0072] In order to enable the above implementation details and operations of the present application to be clearly understood by those skilled in the art, and to demonstrate the significant improvement in the performance of the process for preparing ferric nitrate by leaching iron resources in the embodiment of the present application, the above technical solution is illustrated by multiple embodiments below.

[0073] Example 1

[0074] A red iron leaching process, as shown in the following Figure 2 As shown, the following steps are included:

[0075] 1. Take 50g of red iron oxide and grind it into a powder with a particle size of no more than 23μm (passing 600 mesh). The iron content in the red iron oxide is 69.57% (the purity of the red iron oxide is 99.3%).

[0076] 2. Add 20 g of carbon powder (passing 600 mesh) with a particle size of no more than 23 μm to the iron red in step 1, put it into a ball mill and mill it for 3 hours to obtain precursor 1;

[0077] 3. Add 400 g of nitric acid with a concentration of 68% to the precursor 1 of step 2, set the heating temperature to 90° C., the stirring speed to 500 rpm, and heat and leach for 12 hours to obtain a leaching mixture 1;

[0078] 4. Filter the mixed solution 1 in step 3 to obtain 397.1 g of leachate (i.e., ferric nitrate solution) with an iron content of 8.50% (obtained by inductively coupled plasma ICP or iron titration test), 20.58 g of filter residue (unreacted red iron oxide + carbon powder) with an iron content of 11.02%, calculated as follows: filter residue iron content = ((iron red mass * iron red iron content) - (leachate mass * iron concentration)) / total mass of filter residue.

[0079] According to the formula of iron recovery rate = (leaching solution mass * iron concentration) / (iron red mass * iron red iron content), it is calculated that the iron recovery rate in the leaching solution is 96.74%, and the iron recovery rate in the leaching residue is 3.26%. The details are shown in Table 1 below:

[0080] Table 1

[0081]

[0082] 5. After the leaching residue is digested with hydrochloric acid, according to the data of the leaching solution and the leaching residue, the leaching residue contains 1.63g of unreacted iron oxide red and 18.59g of unreacted carbon powder. To leach the next batch of 50g of iron oxide red, 1.41g of new carbon powder needs to be added, and the amount of iron oxide red needs to be reduced by 1.63g;

[0083] 6. Recycling of leached residue: Add 48.37 g of iron oxide red and 1.41 g of carbon powder to the leached residue in step 5, ball mill for 6 h, add 400 g of 68% nitric acid, heat and leach for 12 h under the same conditions, and the calculated iron oxide red leaching rate is 97.13%, which is basically consistent with the first leaching.

[0084] Example 2

[0085] A red iron leaching process comprises the following steps:

[0086] 1. Take 50g of red iron oxide and grind it into a powder with a particle size of no more than 23μm (passing 600 mesh). The iron content in the red iron oxide is 69.57% (the purity of the red iron oxide is 99.3%).

[0087] 2. Add 20 g of titanium dioxide (600 mesh) with a particle size of no more than 23 μm to the iron red in step 1, put it into a ball mill and mill it for 3 hours to obtain precursor 1;

[0088] 3. Add 400 g of nitric acid with a concentration of 68% to the precursor 1 of step 2, set the heating temperature to 90° C., the stirring speed to 500 rpm, and heat and leaching for 12 h to obtain a leaching mixture 1;

[0089] 4. Filter the mixed solution 1 in step 3 to obtain 401.77 g of leachate (ferric nitrate solution) with an iron content of 8.37% (obtained by inductively coupled plasma ICP or iron titration test), and 21.65 g of filter residue (unreacted red iron oxide + titanium dioxide) with an iron content of 10.60%, which is calculated as follows: filter residue iron content = ((iron red mass * iron red iron content) - (leachate mass * iron concentration)) / total mass of filter residue;

[0090] According to the formula of iron recovery rate = (leaching solution mass * iron concentration) / (iron red mass * iron red iron content), it is calculated that the iron recovery rate in the leachate is 96.7%, and the iron recovery rate in the leaching residue is 3.3%. The details are shown in Table 2 below:

[0091] Table 2

[0092]

[0093] 5. After the leached residue is digested with hydrochloric acid, according to the data of the leaching solution and the leached residue, the leached residue contains 1.65g of unreacted iron oxide and 20g of unreacted titanium dioxide. The next batch of iron oxide leaching does not need to be supplemented with new carbon powder, but the amount of iron oxide needs to be reduced by 1.65g;

[0094] 6. Recycling of leached residue: Add 48.35 g of iron oxide red to the leached residue in step 5, ball mill for 3 h, add 400 g of 68% nitric acid, heat and leach for 12 h under the same conditions, and calculate the iron oxide red leaching rate of 97.25%, which is basically consistent with the first leaching.

[0095] Example 3

[0096] A ferroferric oxide leaching process comprises the following steps:

[0097] 1. Take 50g of ferroferric oxide and grind it into powder with a particle size of no more than 74μm (passing 200 meshes). The iron content in ferroferric oxide is 72.15% (the purity of ferroferric oxide is converted to 99.87%).

[0098] 2. Add 20 g of carbon powder (with a particle size of no more than 74 μm) (passing 200 mesh) to the ferroferric oxide in step 1, and place in a ball mill for 3 h to obtain a precursor 1;

[0099] 3. Add 450 g of nitric acid with a concentration of 68% to the precursor 1 of step 2, set the heating temperature to 90° C., the stirring speed to 600 rpm, and heat and leaching for 14 hours to obtain a leaching mixture 1;

[0100] 4. Filter the mixed solution 1 in step 3 to obtain 451.77 g of leachate (ferric nitrate solution) with an iron content of 7.95% (obtained by inductively coupled plasma ICP or iron titration test); 18.6 g of filter residue (unreacted ferroferric oxide + carbon powder) with an iron content of 0.81%, which is calculated as follows: filter residue iron content = ((iron red mass * iron red iron content) - (leachate mass * iron concentration)) / total mass of filter residue;

[0101] According to the formula of iron recovery rate = (leaching solution mass * iron concentration) / (iron red mass * iron red iron content), it is calculated that the iron recovery rate in the leaching solution is 99.58%, and the iron recovery rate in the leaching residue is 0.42%. The details are shown in Table 3 below:

[0102] Table 3

[0103]

[0104] 5. After the leaching residue is digested with hydrochloric acid, according to the data of the leaching solution and the leaching residue, the leaching residue contains 0.21g of unreacted ferroferric oxide and 18.4g of unreacted carbon powder. For the leaching of the next batch of iron red, 1.6g of new carbon powder needs to be added, and the amount of ferroferric oxide used needs to be reduced by 0.21g;

[0105] 6. Recycling of leached residue: Add 49.79 g of ferroferric oxide and 1.6 g of carbon powder to the leached residue in step 5, ball mill for 3 h, add 450 g of 68% nitric acid, heat and leach for 14 h under the same conditions, the leaching rate of ferroferric oxide is 99.79%, which is basically the same as the first leaching.

[0106] Example 4

[0107] A magnetite leaching process comprises the following steps:

[0108] 1. Take 50g of magnetite concentrate and grind it to a particle size of no more than 74μm powder (passing 200 mesh). The iron content in the magnetite is 72.15%;

[0109] 2. Add 25 g of carbon powder (passing 200 mesh) with a particle size of no more than 74 μm to the magnetite in step 1, and put it into a ball mill for 4 hours to obtain precursor 1;

[0110] 3. Add 400 g of nitric acid with a concentration of 68% to the precursor 1 of step 2, set the heating temperature to 90° C., the stirring speed to 600 rpm, and heat and leach for 14 h to obtain a leaching mixture 1;

[0111] 4. Filter the mixed solution 1 in step 3 to obtain 403.21 g of leachate (ferric nitrate solution) with an iron content of 8.71% (obtained by inductively coupled plasma ICP or iron titration test), and 24.87 g of filter residue (unreacted magnetite + carbon powder) with an iron content of 3.84%, which is calculated as follows: filter residue iron content = ((iron red mass * iron red iron content) - (leachate mass * iron concentration)) / total mass of filter residue;

[0112] According to the formula of iron recovery rate = (leaching solution mass * iron concentration) / (iron red mass * iron content of iron red), it is calculated that the iron recovery rate in the leachate is 97.35%, and the iron recovery rate in the leaching residue is 2.65%. The details are shown in Table 4 below:

[0113] Table 4

[0114]

[0115] 5. After the leaching residue is digested with hydrochloric acid, according to the data of the leaching solution and the leaching residue, the leaching residue contains 1.324g of unreacted iron concentrate and 23.55g of unreacted carbon powder. For the leaching of the next batch of iron red, 1.45g of new carbon powder needs to be added and the amount of magnetite used needs to be reduced by 1.324g;

[0116] 6. Recycling of leached residue: Add 48.676 g of magnetite and 1.45 g of carbon powder to the leached residue in step 5 and ball-mill for 4 h. Add 400 g of 68% nitric acid and heat and leach for 14 h under the same conditions. The leaching rate of magnetite is 98.04%, which is basically the same as the first leaching.

[0117] Example 5

[0118] A red iron leaching process comprises the following steps:

[0119] 1. Take 50g of red iron oxide and grind it into a powder with a particle size of no more than 23μm (passing 600 mesh). The iron content in the red iron oxide is 69.57% (the purity of the red iron oxide is 99.3%).

[0120] 2. Add 20 g of carbon powder (passing 600 mesh) with a particle size not higher than 23 μm and 20 g of manganese dioxide with a particle size not higher than 23 μm to the iron red in step 1, put into a ball mill and mill for 3 hours to obtain a precursor 1;

[0121] 3. Add 400 g of nitric acid with a concentration of 68% to the precursor 1 of step 2, set the heating temperature to 90° C., the stirring speed to 500 rpm, and heat and leach for 12 hours to obtain a leaching mixture 1;

[0122] 4. Filter the mixed solution 1 in step 3 to obtain 389.12 g of leachate (i.e., ferric nitrate solution) with an iron content of 8.66% (obtained by inductively coupled plasma ICP or iron titration test), and 22.71 g of filter residue (unreacted red iron oxide + carbon powder + manganese dioxide) with an iron content of 4.79%, which is calculated as follows: filter residue iron content = ((iron red mass * iron red iron content) - (leachate mass * iron concentration)) / total mass of filter residue;

[0123] According to the formula of iron recovery rate = (leaching solution mass * iron concentration) / (iron red mass * iron red iron content), it is calculated that the iron recovery rate in the leachate is 96.87%, and the iron recovery rate in the leaching residue is 3.16%. The details are shown in Table 5 below:

[0124] Table 5

[0125]

[0126] 5. After the leaching residue was digested with hydrochloric acid, according to the data of the leaching solution and the leaching residue, the leaching residue contained 1.563g of unreacted iron oxide, 18.55g of unreacted carbon powder, and 2.6g of unreacted manganese dioxide (the reason for the consumption of 17.4g of manganese dioxide is that the carbon powder will also participate in the reduction reaction of nitric acid and manganese dioxide, resulting in the loss of manganese dioxide catalyst. The reducing agent and catalyst cannot improve the leaching rate of iron, and will also cause the loss of the catalyst). For the leaching of the next batch of 50g of iron oxide, 1.45g of new carbon powder needs to be added, and the amount of iron oxide used is reduced by 1.563g;

[0127] 6. Recycling of leached residue: Add 48.43 g of iron oxide red, 1.45 g of carbon powder, and 17.4 g of manganese dioxide to the leached residue in step 5, ball mill for 6 h, add 400 g of 68% nitric acid, heat and leach for 12 h under the same conditions, and the calculated iron oxide red leaching rate is 97.97%, which is basically consistent with the first leaching.

[0128] Control test example 1

[0129] A red iron leaching process comprises the following steps:

[0130] 1. Take 50g of red iron oxide and grind it into a powder with a particle size of no more than 23μm (passing 600 mesh). The iron content in the red iron oxide is 69.57% (the purity of the red iron oxide is 99.3%).

[0131] 2. Add 20 g of carbon powder (passing 600 mesh) with a particle size of no more than 23 μm to the iron red in step 1, put it into a ball mill and mill it for 3 hours to obtain precursor 1;

[0132] 3. Add 400 g of nitric acid with concentrations of 40%, 45%, 90%, and 100% to the precursor 1 of step 2, set the heating temperature to 90° C., the stirring speed to 500 rpm, and heat and leach for 12 h to obtain a leached mixed solution 1; filter the mixed solution 1 of step 3 to obtain the leaching solution and the leaching residue yields as shown in Table 6:

[0133] Table 6

[0134]

[0135] Control test example 2

[0136] A red iron leaching process comprises the following steps:

[0137] 1. Take 50g of red iron oxide and grind it into a powder with a particle size of no more than 23μm (passing 600 mesh). The iron content in the red iron oxide is 69.57% (the purity of the red iron oxide is 99.3%).

[0138] 2. Add 20 g of carbon powder (passing 600 mesh) with a particle size of no more than 23 μm to the iron red in step 1, put it into a ball mill and mill it for 3 hours to obtain precursor 1;

[0139] 3. Add 400 g of nitric acid with a concentration of 68% to the precursor 1 of step 2, set the heating temperatures to 55°C, 60°C, 100°C, and 105°C, respectively, and stir at a speed of 500 rpm. Heat and leach for 12 h to obtain a leached mixed solution 1. Filter the mixed solution 1 of step 3 to obtain the leaching solution and leaching residue yields as shown in Table 7 below:

[0140] Table 7

[0141]

[0142] Control test example 3

[0143] A red iron leaching process comprises the following steps:

[0144] 1. Take 50g of magnetite concentrate and grind it to a particle size of no more than 74μm powder (passing 200 mesh). The iron content in the magnetite is 72.15%;

[0145] 2. Add 0.1 g, 1 g, 10 g, and 50 g of carbon powder (200 mesh) with a particle size not higher than 74 μm to the magnetite in step 1, respectively, put it into a ball mill and mill it for 4 hours to obtain precursor 1;

[0146] 3. Add 400 g of nitric acid with a concentration of 68% to the precursor 1 of step 2, set the heating temperature to 90° C., the stirring speed to 600 rpm, and heat and leach for 14 h to obtain a leached mixed solution 1; filter the mixed solution 1 of step 3 to obtain the leaching solution and the leaching residue yields as shown in Table 8 below:

[0147] Table 8

[0148]

[0149]

[0150] It can be seen from the above-mentioned embodiments and control test examples that the embodiments of the present application use a leaching agent in combination with concentrated nitric acid to efficiently and quickly leach iron oxide sources such as iron red, ferroferric oxide, and magnetite to prepare iron nitrate, especially using a reducing agent carbon powder, which is cheap and easy to obtain, with low consumption (consumption of 1% relative to iron red), and titanium dioxide catalysts basically do not produce losses. Under the premise of lower leaching agent loss, a considerable iron leaching yield can be obtained, and the leaching rate of iron red can reach more than 99%. The leached iron nitrate can be directly used as an iron source for preparing iron phosphate-based positive electrode materials by the liquid phase method, reducing the cost of iron source raw materials for preparing iron phosphate-based positive electrode materials by the liquid phase method. In addition, the leached residue can be recycled, which is economical and environmentally friendly and suitable for industrial applications.

[0151] In addition, by comparing test example 1, it can be seen that when the mass fraction of concentrated nitric acid is 45% to 100%, concentrated nitric acid can react with the mixed material more efficiently and quickly, increase the reduction charge, increase the leaching reaction rate, and increase the leaching recovery rate of ferric nitrate.

[0152] By comparing test example 2, it can be seen that when the leaching reaction temperature is around 100° C., it is beneficial to improve the efficiency of the leaching reaction and ensure the safety and controllability of the reaction.

[0153] By comparing test example 3, it can be seen that when the mass ratio of the iron oxide source to the leaching agent is 100:(1-100), it is beneficial to improve the leaching efficiency of the iron oxide source and control the reaction rate and cost.

[0154] In addition, the process also has good versatility and is suitable for the extraction of iron resources from different iron oxides such as hematite, ferroferric oxide, and magnetite. It has a high iron recovery rate and provides a low-cost hydrometallurgical process route for mineral resources. The process route is short, and the main process only includes mixed ball milling-leaching reaction. Furthermore, by recycling the leaching residue, the recovered unreacted iron source and leaching agent can be reused in the process of leaching iron resources to prepare ferric nitrate, forming a closed loop with few by-products, which is suitable for industrial application.

[0155] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A process for preparing ferric nitrate by leaching iron resources, characterized in that: The following steps are involved: The iron oxide source and the leaching agent are mixed and ground to obtain a mixed material; the leaching agent provides a reducing potential; After the mixed material is mixed with concentrated nitric acid, a leaching reaction is carried out under heating conditions to separate and obtain a leachate and a leach residue, wherein the leachate includes ferric nitrate.

2. The process for preparing ferric nitrate by leaching iron resources as claimed in claim 1, characterized in that: The purity of the ferric nitrate in the leachate is not less than 99.9%; And / or, the leaching solution is directly used as an iron source in the liquid phase method for preparing an iron phosphate-based positive electrode material.

3. The process for preparing ferric nitrate by leaching iron resources as claimed in claim 1 or 2, characterized in that: The iron oxide source includes at least one of iron oxide red, ferroferric oxide, hematite, and magnetite; And / or, the leaching agent includes at least one of a reducing agent and a catalyst.

4. The process for preparing ferric nitrate by leaching iron resources as claimed in claim 3, characterized in that: The reducing agent includes at least one of carbon powder, white phosphorus, sucrose, glucose, acetic acid, formic acid, benzoic acid, and starch; And / or, the catalyst includes at least one of TiO2, MnO2, Pt, Pd, and Rh.

5. The process for preparing ferric nitrate by leaching iron resources according to any one of claims 1 to 2 or 4, characterized in that: The mass ratio of the iron oxide source to the leaching agent is 100:(1-100).

6. The process for preparing ferric nitrate by leaching iron resources as claimed in claim 5, characterized in that: The mixed grinding conditions include: ball milling for 1 h to 10 h at a rotation speed of 600 rpm to 1500 rpm; And / or, the particle size of the particles in the mixed material is 200-1000 mesh.

7. The process for preparing ferric nitrate by leaching iron resources according to any one of claims 1 to 2, 4 or 6, characterized in that: The mass fraction of the concentrated nitric acid is 45% to 100%; And / or, the mass ratio of the mixed material to the concentrated nitric acid is 1:(1-20).

8. The process for preparing ferric nitrate by leaching iron resources as claimed in claim 7, characterized in that: The leaching reaction conditions include: leaching for 6h to 24h at a temperature of 90°C to 150°C and a stirring rate of 300rpm to 800rpm.

9. The process for preparing ferric nitrate by leaching iron resources according to any one of claims 1 to 2, 4, 6 or 8, characterized in that: Also includes the steps: Recycling the leached residue to obtain an incompletely reacted leaching agent; The unreacted leaching agent is recycled and applied to the process of leaching iron resources to prepare ferric nitrate.

10. An application of the process for preparing ferric nitrate by leaching iron resources according to any one of claims 1 to 9, characterized in that: The process of preparing ferric nitrate by leaching the iron resource is applied in the field of lithium-ion batteries.