Method for changing fluorine ion battery electrode material into fluorine ion electro-adsorption electrode and application of fluorine ion battery electrode material

Through bismuth-embedded porous nanocarbon materials as fluoride ion electro-adsorption electrodes, the Faraday effect and electric double-layer capacitors are used to solve the problems of low efficiency and high energy consumption in traditional fluorine removal technology, and achieve high efficiency fluorine ion capture and stability , suitable for pollution control and environmental analysis.

CN118929850APending Publication Date: 2024-11-12ELECTRIC POWER SCI & RES INST OF STATE GRID TIANJIN ELECTRIC POWER CO +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410979575.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional fluorine removal technology is inefficient in removing fluorine ion pollutants, has high energy consumption and is difficult to meet strict emission requirements, and has insufficient understanding of the mechanism of the fluorine ion electrosorption process.

Method used

Using bismuth-embedded porous nanocarbon material (MBiC@tE) as fluoride ion electrosorption electrode, the synergistic effect of Faraday effect and electrical bilayer (EDL) capacitors can achieve efficient fluoride electrosorption, combined with the formation of redox active bismuth By bond reaction, a fluorine ion electro-adsorption electrode with high adsorption capacity and stability was prepared.

Benefits of technology

It has achieved efficient capture of fluorine ions, significantly improved the electro-adsorption capacity and stability of fluorine ions, is suitable for pollution control and environmental analysis, has commercial potential, and provides a foundation for future high-performance Faraday electrode design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929850A_ABST
    Figure CN118929850A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of electrode materials, and discloses a method for changing a fluorine ion battery electrode material into a fluorine ion electro-adsorption electrode and application of the fluorine ion electro-adsorption electrode. And preparing the fluorine ion electro-adsorption electrode. The prepared fluorine ion electro-adsorption electrode has the structural characteristic of multiple pores, is rich in binding sites, has excellent adsorption capacity, can gradually reach absorption equilibrium within about 45 minutes under the concentration of fluorine ions of 100 ppm, and has great potential in the aspects of separation and monitoring of water system fluorine-containing substances in multiple fields of environmental pollution control and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode material preparation, and in particular to a method for converting a fluoride ion battery electrode material into a fluoride ion electrosorption electrode and a use thereof. Background Art

[0002] Rapid population growth and rapid industrialization have prompted efforts to alleviate water shortages and repair polluted water environments to address major obstacles to sustainable development. Among the various pollutants in natural water, the generally high concentration of fluoride ions has become a major problem due to its adverse effects on human health. The hazards associated with excessive fluoride intake manifest as fluorosis of teeth and bones, and can develop into arthritis and disabling brittle bone disease. However, traditional fluoride removal technologies are limited by removal efficiency, secondary pollution and high energy consumption, making it difficult to meet increasingly stringent emission requirements.

[0003] Recently, electro-assisted adsorption (or electrosorption) technology has shown excellent performance in separating ionic pollutants, with advantages such as high energy efficiency, low environmental impact and low cost. Specifically, electrolyte ions are transported into the nanopores of electroactive electrode materials to achieve the capture of pollutant ions. Compared with traditional adsorption methods, by applying a potential difference between the electrodes, the interaction of pollutant anions during the transfer process and their binding strength with the active material can be adjusted, thereby achieving high capacity.

[0004] The capacity of electrosorption systems is significantly affected by the characteristics of the electrode materials. Nanoporous carbon materials are most widely used in the environmental and energy fields due to their structural flexibility and optimized diffusion processes. Recently, faradaic redox materials have been discovered in fluoride ion batteries (FIBs) that show greater charge storage capacity and energy-efficient reversible fluorination / defluorination due to the formation of metal fluoride layers. The morphological evolution of these materials during defluorination indicates that they have high faradaic pseudocapacitance according to the redox reaction principle. Since ion exchange has reached its limit according to the electrical double layer (EDL) theory, the development of porous carbon materials containing redox-active bismuth to reversibly form insoluble bismuth fluoride will have the potential to overcome the capacity limitation of common ion exclusion during fluoride electrosorption. However, the fundamental understanding of the impact of redox processes on charge transfer and, in turn, the characteristics and mechanisms of fluoride electrosorption is still insufficient.

[0005] Therefore, a novel composite electrode with redox-active bismuth nanoparticles encapsulated in a porous carbon matrix was prepared and applied to efficient fluoride electrosorption via the synergistic effect of the Faraday effect and EDL capacitance. Significantly superior electrosorption capacity and electrosorption rate were exhibited in the Faraday effect-dominated electro-assisted fluoride adsorption process. More importantly, a comprehensive understanding of the electrosorption behavior of bismuth-deposited materials was proposed through a series of experiments and characterizations, which will guide the design of high-performance Faraday electrodes in the future. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method and use of converting a fluoride ion battery electrode material into a fluoride ion electrosorption electrode. The fluoride ion electrosorption electrode has a large adsorption capacity and maintains good stability under the condition of coexisting ions. It can be used as a sample pretreatment medium in the fields of pollution control and environmental analysis.

[0007] The technical solution adopted by the present invention to solve the technical problem is:

[0008] In one aspect, the present invention provides a method for converting a fluoride ion battery electrode material into a fluoride ion electrosorption electrode, comprising the following steps:

[0009] (1) Preparation of bismuth-embedded porous carbon material MBiC@tE: Bi(NO3)3-5H2O) and trimesic acid (H3BTC) were added to a methanol solution and dissolved and stirred, and then the solution was transferred to an ultrasonic bath and kept at room temperature for 30-60 minutes to obtain a first reaction solution;

[0010] The first reaction liquid is poured into a reactor with a polytetrafluoroethylene substrate, and maintained at 110-120° C. for 22-26 hours to obtain a second reaction liquid, and the second reaction liquid is taken out and a white precipitate is obtained by vacuum filtration, which is washed with methanol and dried in an oven at 50-70° C. overnight to obtain a dry Bi-MOF precursor (MOFBi);

[0011] The dried Bi-MOF precursor was evenly ground and placed in a tube furnace, heated to 700-900°C at a rate of 4-6°C / min under a nitrogen atmosphere, and kept at 700-900°C for 220-260 minutes for full carbonization to obtain a bismuth-embedded porous nanocarbon material (MBiC@tE);

[0012] (2) Preparation of fluoride ion electrosorption electrode: The bismuth-embedded porous nanocarbon material (MBiC@tE) is dispersed with conductive carbon black and PTFE in an ethanol solution, mixed with an agate mortar to obtain a pre-made slurry, and the pre-made slurry is evenly coated on graphite paper. The graphite paper is dried at 50-70° C. overnight to obtain a fluoride ion electrosorption electrode.

[0013] Furthermore, the volumetric dosage of the methanol and the mass ratio of bismuth nitrate pentahydrate are 55-65 mL: 0.13-0.17 g.

[0014] Furthermore, the mass ratio of the bismuth nitrate pentahydrate to trimesic acid is 1:4.8-1:5.2.

[0015] Furthermore, the mass ratio of the bismuth-embedded porous nanocarbon material (MBiC@tE): conductive carbon black: PTFE is 8:1:1.

[0016] On the other hand, the present invention provides an application of the fluoride ion electrosorption electrode prepared by the method for electrosorption in a sodium fluoride solution, wherein the fluoride ion electrosorption electrode is an anode, and carboxyl activated carbon is used as a cathode counter electrode. The electrosorption process is carried out in a sodium fluoride solution under the condition of an applied voltage. After the electrosorption process is completed, the treated sodium fluoride solution is taken and the residual fluoride ion content is measured using an ultraviolet spectrophotometer.

[0017] Furthermore, the pH of the fluoride ion electrosorption electrode was adjusted to 6.7±7.3 before the electrosorption process with simulated wastewater containing fluoride ions.

[0018] Furthermore, the electrosorption time of the fluoride ion electrosorption electrode and the simulated wastewater containing fluoride ions is 15-45 minutes.

[0019] Furthermore, the fluoride ion concentration in the sodium fluoride solution is 10-100 mg / L.

[0020] Furthermore, the applied potential during the electrosorption process is 0-1.4V.

[0021] The preparation method of the fluoride ion electrosorption electrode of the present invention realizes the embedding of bismuth redox active units in porous nano-carbon materials. The fluoride ion electrosorption electrode has a nano-rod-shaped main structure and loads sufficient internal active sites.

[0022] The bismuth-embedded porous nanocarbon material (MBiC@tE) of the present invention, wherein the Bi-MOF precursor has a relatively smooth surface, is subjected to carbonization treatment to obtain a bismuth-embedded redox-active porous carbon material, and efficient electrically assisted capture of fluoride ions is achieved based on the bonding reaction between bismuth and fluorine, showing high adsorption capacity and high stability in simulated wastewater treatment projects.

[0023] The bismuth-embedded porous nanocarbon material MBiC@tE of the present invention is obtained by annealing the previously prepared Bi-MOF precursor at 700-900 degrees Celsius. It well retains the structure of the Bi-MOF precursor and shows obvious advantages in surface morphology.

[0024] The fluoride ion electrosorption electrode of the present invention exhibits excellent fluoride ion capturing performance, excellent stability and outstanding adsorption rate, and exhibits excellent performance in the process of separating and enriching fluoride ions in wastewater.

[0025] The electrode material of the present invention has been subjected to a series of characterizations such as XPS, XRD, BET, FT-IR, TGA, SEM, etc. in order to verify the above-mentioned unique structural engineering design, and the feasibility of the structure, the effectiveness of the synthesis, and the real existence of the chemical components have been proved from the microstructure. In addition, in control experiments with different reaction conditions, on the basis of traditional EDL double-layer electrosorption, the adsorption behavior of the electrode material of the present invention is strongly affected by the Faraday electrochemical reaction. Through the analysis of XRD and XPS test results, the electrode material after adsorption shows the characteristic peak type of BiF3, which explains the phase change of the chemical components caused by the conversion reaction, which provides sufficient data for various model comparisons, thereby enriching the defluorination mechanism.

[0026] In the electrode material prepared by the present invention, the fluoride has enough time to contact with bismuth to undergo controlled reversible transformation, highlighting the potential for the development of the redox phase change mechanism driven by charge compensation, thereby achieving efficient adsorption of fluorine. It can achieve a strong enrichment ability for fluoride ions, so it has great potential in the separation and monitoring of fluorine-containing substances in water systems in multiple fields such as environmental pollution control.

[0027] The advantages and beneficial effects of the present invention are:

[0028] The electrode material of the present invention, under the stimulation of the applied potential difference, electron transfer triggers the intermediate metastable Bi 2+ The formation of trivalent bismuth fluoride eventually results from the inherent affinity of bismuth for fluorine, which maintains excellent fluoride ion recognition performance, stable physicochemical properties, clear preparation process, and can be synthesized on a large scale. By combining with other pretreatment processes, its application range can be further expanded.

[0029] The electrode material of the present invention has a porous structural feature, rich binding sites, significant double synergistic effect, and large capacity and high adsorption rate, which ensure the feasibility of enriching fluoride ions.

[0030] The electrode material of the present invention has fast binding kinetics and strong adsorption capacity. It can gradually reach absorption equilibrium in about 45 minutes at a concentration of 100 ppm. The excellent adsorption capacity and rapid adsorption equilibrium give this material extraordinary commercial potential.

[0031] The electrode material of the present invention specifically analyzes the phase change reaction process between bismuth and fluorine, providing inspiration for the future design of other high-performance fluorine removal systems.

[0032] The defluorination process is effectively controlled by the electrochemical process. The fluoride removal capacity is partly due to the surface-controlled EDL capacitance. This electrically controlled reversible Faradaic reaction based on the binding between bismuth and fluoride also enhances the diffusion-controlled pseudocapacitance. The electrochemically controlled dual-mode coupling process achieves rapid electrosorption of fluoride. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 N2 adsorption / desorption isotherms of the electrode materials MBiC@tS, MBiC@tN, MBiC@tE, and MOFBi prepared in accordance with the embodiments of the present invention;

[0034] Figure 2 The pore size distribution of the electrode materials MBiC@tS, MBiC@tN, MBiC@tE, and MOFBi prepared in the embodiments of the present invention;

[0035] Figure 3 Infrared characterization images of the electrode materials MC@tE, MBiC@tS, MBiC@tN, MBiC@tE, and MOFBi prepared in the embodiments of the present invention;

[0036] Figure 4 The voltammetric cycle curve of the electrode material MBiC@tE prepared in the embodiment of the present invention;

[0037] Figure 5 X-ray photoelectron spectroscopy characterization diagrams of the electrode materials MC@tE, MBiC@tS, MBiC@tN, MBiC@tE, and MOFBi prepared in the embodiments of the present invention;

[0038] Figure 6 Adsorption capacity diagram of electrode materials MC@tE, MBiC@tS, MBiC@tN, MBiC@tE, and MOFBi prepared in the embodiments of the present invention for fluorine-containing wastewater of different concentrations;

[0039] Figure 7 X-ray diffraction characterization diagrams of the electrode materials MC@tE, MBiC@tS, MBiC@tN, MBiC@tE, and MBiC@tE-absorbed prepared in the embodiments of the present invention;

[0040] Figure 8 Schematic diagram of the adsorption process of the electrode material prepared in an embodiment of the present invention;

[0041] Fig. 9 Schematic diagram of the preparation process and application of the electrode material according to an embodiment of the present invention. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0043] Example 1

[0044] A method for converting a fluoride ion battery electrode material into a fluoride ion electrosorption electrode comprises the following steps:

[0045] (1) Preparation of bismuth-embedded porous carbon material MBiC@tE: A two-step strategy was adopted, including an organic hydrothermal method and a slightly modified N2 atmosphere annealing treatment, in which interfacial coupling was achieved between Bi(NO3)3-5H2O and trimesic acid (H3BTC). Specifically, 0.75 g 1,3,5-benzenetricarboxylic acid and 0.15 g Bi(NO3)3-5H2O were added to 60 mL methanol, and the mixture was dissolved by ultrasonication at room temperature for 15 minutes to form an opaque white solution, which was the first reaction solution. The treated first reaction solution was then transferred and sealed into a 100 mL Teflon-lined steel reactor, heated at 120°C for 24 hours and naturally cooled to room temperature to obtain the second reaction solution. A white precipitate (called MOFBi) was obtained by vacuum filtration. The collected white precipitate was washed with methanol several times and then dried in an oven at 60°C for 10 hours to obtain the dry Bi-MOF precursor MOFBi.

[0046] The dried precursor (MOFBi) was transferred to a tube furnace and annealed and carbonized at 800 °C in a nitrogen environment for 4 h with a heating rate of 5 °C / min. After annealing, the synthesized powder (denoted as MBiC@tE) was washed three times with distilled water to remove impurities and then dried at 60 °C to obtain bismuth-embedded porous nanocarbon material MBiC@tE;

[0047] (2) Preparation of fluoride ion electrosorption electrode: The bismuth-embedded porous nanocarbon material MBiC@tE, conductive carbon black, and polytetrafluoroethylene were dispersed in 0.02 g of ethanol at a mass ratio of 8:1:1. The mixture was fully ground with an agate mortar to obtain a pre-made slurry, and then the pre-made slurry was evenly coated on the lower half of a 7×3 square centimeter graphite paper, accounting for about 40% of the graphite paper. The bonding effect was ensured by rolling, and then the coated paper was dried at 60°C overnight to obtain a fluoride ion electrosorption electrode.

[0048] The voltammetric cycle curves of the fluoride ion electrosorption electrode prepared in Example 1 at different voltages are shown in FIG. Figure 4 shown.

[0049] Application Example 1

[0050] Application of the fluoride ion electrosorption electrode prepared in Example 1 in electrosorption of sodium fluoride solution:

[0051] The sodium fluoride solution was sodium fluoride simulated wastewater, and MBiC@tE was used as a fluoride ion capture electrode. Carboxyl activated carbon was used as the cathode counter electrode. Under room temperature conditions, the electrosorption process was carried out at a voltage of 1.2V in a fixed bed closed reactor to test the fluoride removal performance, and the initial fluoride ion concentrations were 10mg / L, 50mg / L and 100mg / L.

[0052] The average of the results of three parallel experiments was used to determine the reliable experimental data. The solution after adsorption was taken and the remaining fluoride ion content in the supernatant was measured and analyzed using an ultraviolet spectrophotometer at 620 nm.

[0053] The contributions of capacitive charge and diffusion-controlled charge in the summary graph are calculated using the following equations:

[0054] i(v)=av k (1)

[0055] log(i)=blog(v)+log(a)(Replacek with b) (2)

[0056] i(v)=k1v+k2v 0.5 (3)

[0057] In addition, the effects of pH and coexisting anions on the adsorption performance were also investigated.

[0058] The adsorption capacity of the adsorbent at different concentrations was calculated. Figure 6 , the calculation formula is as follows:

[0059]

[0060] It is calculated that at an initial fluorine concentration of 100 mg / L, the adsorption capacity is above 38.98 mg / g (in terms of fluoride ions).

[0061] The experiment showed that when the initial fluorine concentration was 100 mg / L, the adsorbent reached adsorption saturation in about 45 minutes.

[0062] The electrode exhibits the best fluoride removal performance under neutral conditions, which is attributed to the formation of insoluble BiF3. In contrast, under acidic conditions, the oxidation products of bismuth exist in ionic form, which leads to an insurmountable reaction barrier and significantly reduces the fluoride ion electrosorption capacity. As the pH value increases to alkaline conditions, hydroxide ions occupy the active sites of the bismuth deposited material, thereby competitively inhibiting the ligand exchange behavior that dominates fluoride removal.

[0063] The coexisting ions also affect the performance of the adsorbent. The significant decrease in fluoride removal indicates that CO3 2- and HCO 3-It may cause electrode scaling. Cl- competes with fluoride for active sites in the secondary reaction, which ultimately leads to a significant decrease in adsorption capacity. 2- and PO4 3- The diffusion of fluoride is hindered by the rapid accumulation and common ion effect on the electrode with higher valence. On the contrary, due to the high electronegativity of fluoride, NO 3- The presence of has no significant inhibitory effect on the removal of fluoride.

[0064] Example 2

[0065] (1) Preparation of bismuth-embedded porous carbon material MBiC@tE: A two-step strategy was adopted, including an organic hydrothermal method and a slightly modified N2 atmosphere annealing treatment, in which interfacial coupling was achieved between Bi(NO3)3-5H2O and trimesic acid (H3BTC). Specifically, 0.75g 1,3,5-benzenetricarboxylic acid and 0.17g Bi(NO3)3-5H2O were added to 55mL methanol, and the mixture was dissolved by ultrasonication at room temperature for 15 minutes to form an opaque white solution, which was the first reaction solution. The treated first reaction solution was then transferred and sealed into a 100mL Teflon-lined steel reactor, heated at 120°C for 24 hours and naturally cooled to room temperature to obtain the second reaction solution. A white precipitate (called MOFBi) was obtained by vacuum filtration. The collected white precipitate was washed with methanol several times and then dried in an oven at 60°C for 10 hours to obtain the dry Bi-MOF precursor MOFBi.

[0066] The dried precursor (MOFBi) was transferred to a tube furnace and annealed and carbonized at 800 °C in a nitrogen environment for 3.5 h with a heating rate of 6 °C / min. After annealing, the synthesized powder (denoted as MBiC@tE) was washed three times with distilled water to remove impurities and then dried at 70 °C to obtain bismuth-embedded porous nanocarbon material MBiC@tE;

[0067] (3) Preparation of fluoride ion electrosorption electrode: The bismuth-embedded porous nanocarbon material MBiC@tE, conductive carbon black, and polytetrafluoroethylene were dispersed in 0.05 g of ethanol at a mass ratio of 8:1:1. The mixture was fully ground with an agate mortar to obtain a pre-made slurry, and then the pre-made slurry was evenly applied to the lower half of a 7×3 square centimeter graphite paper, accounting for about 40% of the graphite paper. The bonding effect was ensured by rolling, and then the coated paper was dried at 60°C overnight to obtain a fluoride ion electrosorption electrode.

[0068] Application Example 2

[0069] The fluoride ion electrosorption electrode prepared in Example 2 was applied for electrosorption in sodium fluoride solution. The specific steps were the same as those in Application Example 1. The initial fluoride ion concentrations were 100 mg / L, 10 mg / L and 5 mg / L, and the fluoride ion concentrations after adsorption were 93 mg / L, 7.8 mg / L and 2.5 mg / L.

[0070] Comparative Example 1

[0071] The dried precursor (MOFBi) was transferred to a tube furnace and annealed and carbonized at 700 °C in a nitrogen environment for 4 h with a heating rate of 5 °C / min. After annealing, the synthesized powder (denoted as MBiC@tS) was washed three times with distilled water to remove impurities and then dried at 60 °C to obtain bismuth-embedded porous nanocarbon material MBiC@tS;

[0072] Comparative Example 2

[0073] The dried precursor (MOFBi) was transferred to a tube furnace and annealed and carbonized at 900 °C in a nitrogen environment for 4 h with a heating rate of 5 °C / min. After annealing, the synthesized powder (denoted as MBiC@tN) was washed three times with distilled water to remove impurities and then dried at 60 °C to obtain bismuth-embedded porous nanocarbon material MBiC@tN;

[0074] Comparative Example 3

[0075] Add 0.25g of bismuth-embedded porous nanocarbon material MBiC@tE to 100ml of 2.95mol / L hydrochloric acid, stir at room temperature for 240 minutes, pour the reaction solution into vacuum filtration and wash the black solid particles with hydrochloric acid and deionized water, and dry the obtained black solid particles at 60 degrees to obtain MC@tE.

[0076] Characterization and testing

[0077] The sodium fluoride solution was sodium fluoride simulated wastewater, and MBiC@tN, MBiC@tS, MOFBi and MC@tE were used as fluoride ion capture electrodes. Carboxyl activated carbon was used as the cathode counter electrode. Under room temperature conditions, the electrosorption process was carried out at a voltage of 1.2V in a fixed bed closed reactor to test the fluoride removal performance, and the initial fluoride ion concentration was 100mg / L.

[0078] The average of the results of three parallel experiments was used to determine the reliable experimental data. The adsorbed solution was measured using an ultraviolet spectrophotometer at 620 nm, and the amount of fluoride ion removed per gram of electrode material was analyzed. The removal capacity was not as good as that of MBiC@tE.

[0079] The performance of the electrode materials prepared in Example 1 and Comparative Examples 1-3 was tested respectively. The N2 adsorption / desorption isotherm curves are shown in FIG. Figure 1As shown, it can be seen from the figure that the carbonized material retains the carbon nano-confined bismuth configuration presented by the precursor, and at the same time exhibits a suitable pore structure for regulating the mass transfer process.

[0080] Pore ​​size distribution Figure 2 As shown in the figure, it can be seen that the pore size is concentrated in 2-10nm, which is a mesoporous material.

[0081] Infrared characterization Figure 3 As shown in the figure, it can be seen that 1590cm -1 The absorption peak at 1452 cm corresponds to the stretching vibration of the C=O bond, while the absorption peak at 1452 cm -1 and 1397cm -1 The peaks at 845 cm-1 are related to the asymmetric and symmetric vibrations of the carboxyl group, respectively. -1 The peak at 536 cm corresponds to the bending vibration of the CH bond in the benzene ring, while the peak at 536 cm -1 The peak at 654–500 cm -1 The absorption peak at 240 nm changes significantly due to the formation of other bismuth-based compounds (such as BiF3).

[0082] X-ray photoelectron spectroscopy characterization Figure 5 As shown, the coexistence of C, Bi and O species in the composite material can be seen, indicating the successful anchoring of Bi.

[0083] Figure 6 The adsorption capacity of electrode materials MC@tE, MBiC@tS, MBiC@tN, MBiC@tE, and MOFBi for fluorine-containing wastewater of different concentrations. It can be seen from the figure that MBiC@tE reaches electrical adsorption equilibrium (about 40.3 mg g) in about 45 minutes. -1 ), with a maximum rate of 1.4 mgg -1 min -1 Compared with other materials, the optimal carbonization degree improves the ion electrosorption capacity of MBiC@tE in fluoride-rich water environment.

[0084] Figure 7X-ray diffraction characterization diagrams of electrode materials MC@tE, MBiC@tS, MBiC@tN, MBiC@tE, and MBiC@tE-absorbed electrodes after adsorption of fluoride ions. It can be seen from the figure that for MBiC@tS, MBiC@tN, and MBiC@tE, two Bi-based materials, hexagonal Bi (JCPDS No. 85-1329) and its oxide (JCPDS No. 78-1793), successfully indexed all bends in the XRD spectrum. The absence of obvious characteristic peaks after acid washing (MC@tE) indicates that there is no Bi / Bi2O3 on the material. The three significant new diffraction peaks at 25.6°, 38.2°, and 42.7° confirm the removal of this specific form of fluoride, which is related to BiF3 (JCPDS No. 15-0053), and the weakening of the characteristic signals of Bi and Bi2O3 after the adsorption is also proved.

[0085] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept, which all belong to the protection scope of the present invention.

Claims

1. A method for converting a fluoride ion battery electrode material into a fluoride ion electrosorption electrode, characterized in that: The steps include: (1) Preparation of bismuth-embedded porous carbon material: bismuth nitrate pentahydrate and trimesic acid were added to a methanol solution and dissolved and stirred, and then the solution was transferred to an ultrasonic bath and kept at room temperature for 30-60 minutes to obtain a first reaction solution; The first reaction liquid is poured into a reactor with a polytetrafluoroethylene substrate, and maintained at 110-120° C. for 22-26 hours to obtain a second reaction liquid, and the second reaction liquid is taken out and a white precipitate is obtained by vacuum filtration, which is washed with methanol and dried in an oven at 50-70° C. to obtain a dry Bi-MOF precursor; The dried white powder Bi-MOF precursor is ground evenly and placed in a tube furnace, heated to 700-900°C at a rate of 4-6°C / min in a nitrogen atmosphere, and kept at 700-900°C for 220-260 minutes for full carbonization to obtain a bismuth-embedded porous nanocarbon material; (2) Preparation of fluoride ion electrosorption electrode: The bismuth-embedded porous nanocarbon material, conductive carbon black and PTFE are dispersed in an ethanol solution, mixed with an agate mortar to obtain a pre-made slurry, and the pre-made slurry is evenly coated on graphite paper. The graphite paper is dried at 50-70° C. overnight to obtain a fluoride ion electrosorption electrode.

2. The method according to claim 1, characterized in that: The volumetric dosage of the methanol and the mass ratio of bismuth nitrate pentahydrate are 55-65 mL: 0.13-0.17 g.

3. The method according to claim 1, characterized in that The mass ratio of the bismuth nitrate pentahydrate to trimesic acid is 1:4.8-1:5.

2.

4. The method according to claim 1, characterized in that: The mass ratio of the bismuth-embedded porous nanocarbon material: conductive carbon black: PTFE described in step (2) is 8:1:

1.

5. Application of the fluoride ion electrosorption electrode prepared by the method according to any one of claims 1 to 4 in electrosorption in sodium fluoride solution, characterized in that: The fluoride ion electrosorption electrode is used as the anode, and carboxyl activated carbon is used as the cathode counter electrode. The electrosorption process is carried out in a sodium fluoride solution under the condition of an applied voltage. After the electrosorption process is completed, the adsorbed sodium fluoride solution is taken and the residual fluoride ion content is measured using an ultraviolet spectrophotometer.

6. The electrosorption application according to claim 5, characterized in that: The pH of the fluoride ion electrosorption electrode was adjusted to 6.7-7.3 before the electrosorption process with simulated wastewater containing fluoride ions.

7. The electrosorption application according to claim 5, characterized in that: The electrosorption time of the fluoride ion electrosorption electrode and the simulated wastewater containing fluoride ions is 15-45 minutes.

8. The electrosorption application according to claim 5, characterized in that: The fluoride ion concentration in the sodium fluoride solution is 10-100 mg / L.

9. The electrosorption application according to claim 5, characterized in that: The applied potential during the electrosorption process is 0-1.4V.

Citation Information

Cited By

  • Mesoporous electro-adsorption defluorination positive electrode material rich in defects after vulcanization reconstruction