Pearlescent magical-color flash frit and preparation method thereof

The cerium oxide-encapsulated fluorogold mica glassy is formed through raw materials such as perlite, which solves the problem of pearlescent color flash fuse failure and covering pattern at high temperatures, achieves strong and uniform flash effect and high temperature resistance, and expands the application range .

CN118930050AActive Publication Date: 2024-11-12FOSHAN DONGPENG CERAMIC +3
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411034382.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing pearlescent color flash fuses lose their effect at high temperature firing, and the dark iron oxide color can easily cover the pattern of the tile decorative layer, resulting in limited application range.

Method used

The raw materials such as perlite, quartz, alumina, electromelted magnesium sand, potassium fluorosilicate, potassium nitrate and cerium oxide are used to form cerium oxide-encapsulated fluorogold mica glassy by high temperature firing, forming crystals with different refractive indices to form Strong and uniform specular reflection effect and improve the high temperature resistance of fluorogen mica.

Benefits of technology

It realizes the strong pearlescent color flash effect under high temperature firing, does not cover the original pattern of the tiles, expands the application range, and improves the wear resistance and stain resistance of the tiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930050A_ABST
    Figure CN118930050A_ABST
Patent Text Reader

Abstract

The invention discloses a pearlescent colorful flash frit, which is prepared from the following raw materials in parts by mass: 8 to 20 parts of perlite, 25 to 35 parts of quartz, 8 to 15 parts of aluminum oxide, 10 to 18 parts of fused magnesite, 3 to 8 parts of potassium fluosilicate, 8 to 15 parts of potassium nitrate, 5 to 10 parts of phase splitting agent, 5 to 10 parts of cerium oxide and 6 to 16 parts of fluxing agent. According to the pearlescent colorful flashing frit and the preparation method thereof provided by the invention, on the premise of not influencing the pattern effect of the original decorative layer of a ceramic tile, a strong and uniform pearlescent colorful flashing effect can be formed, and the pearlescent colorful flashing effect can be effectively maintained under high-temperature firing, so that the defects in the prior art are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building ceramics, and in particular to a pearlescent colorful flashing frit and a preparation method thereof. Background Art

[0002] In the vast world of the ceramic market, consumers' demands are becoming increasingly diversified and personalized. They not only pursue the practicality and durability of ceramic products, but also have high expectations for their artistic value and visual beauty. This change in market demand has prompted the ceramic industry to continuously innovate technology and develop products to meet the growing aesthetic and practical needs.

[0003] In the production process of ceramic tiles, the mixing of glazes is also extremely important. The same body will produce different glaze effects due to different glazes. The different touch and visual perception of the glaze will also affect the choice of consumers. Pearlescent Magic Flash frit is a special frit. When the glaze with pearlescent magic flash frit is applied to the surface of the body and fired at high temperature, the surface of the tile can present a pearlescent magic flash effect, which not only meets the market demand for the appearance of ceramic tile products, but also provides new ideas and directions for technological innovation and product upgrades in the ceramic industry, avoiding the homogenization of ceramic tile products and increasing the added value of ceramic tile products.

[0004] The existing pearlescent fantasy sparkle frits, due to the differences in the selection of raw materials and the preparation process, most of the produced ceramic tile glazes have technical problems such as weak pearlescent fantasy effect and uneven distribution of flash points. In addition, the prior art generally uses high-refractive index oxides (such as iron oxide) to wrap the surface of low-refractive index mica minerals to form a pearlescent fantasy effect. However, since iron oxide is dark in color and easily turns red, it will cover the original pattern of the ceramic tile decorative layer and affect its decorative effect. In addition, the high-temperature decomposition of mica minerals will easily cause the pearlescent fantasy sparkle frit to no longer have a pearlescent fantasy effect, so that the pearlescent fantasy sparkle frit can only be used under low-temperature calcination conditions. Therefore, the limitations of the above-mentioned factors have led to a very limited scope of application of the existing pearlescent fantasy sparkle frits. Summary of the invention

[0005] The purpose of the present invention is to propose a pearlescent fantasy flash frit and a preparation method thereof, which can not only form a strong and uniform pearlescent fantasy flash effect without affecting the pattern effect of the original decorative layer of the tile, but also effectively maintain its pearlescent fantasy flash effect under high-temperature firing, so as to overcome the shortcomings of the prior art.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] A pearlescent colorful sparkling frit comprises the following raw materials, calculated by weight: 8 to 20 parts of perlite, 25 to 35 parts of quartz, 8 to 15 parts of aluminum oxide, 10 to 18 parts of fused magnesia, 3 to 8 parts of potassium fluorosilicate, 8 to 15 parts of potassium nitrate, 5 to 10 parts of a phase separator, 5 to 10 parts of cerium oxide and 6 to 16 parts of a flux.

[0008] Furthermore, the mesh number of the cerium oxide is 300-325 meshes, the mesh number of the perlite is 300-325 meshes, and the mesh number of the fused magnesia is 380-400 meshes.

[0009] Furthermore, the flux includes zinc oxide and lithium carbonate, and calculated by mass ratio, the mixing ratio of the zinc oxide and the lithium carbonate is (0.8-1.2):1.

[0010] Furthermore, the phase separation agent is calcium phosphate.

[0011] Furthermore, calculated by mass percentage, the chemical composition of the pearlescent colorful sparkling frit includes SiO2 47-48%, Al2O3 19-22%, Fe2O3 0.2-0.5%, CaO 5-6%, MgO 10-12%, K2O 7-8.5%, ZnO4.4-4.5%, Na2O 0.02-0.03%, CeO 6-8% and P2O5 3.5-4.5%.

[0012] Furthermore, calculated by weight, the pearlescent colorful sparkling frit includes the following raw materials: 10 parts of perlite, 32 parts of quartz, 10 parts of alumina, 15 parts of fused magnesia, 5 parts of potassium fluorosilicate, 10 parts of potassium nitrate, 8 parts of a phase separator, 6 parts of cerium oxide and 9 parts of a flux.

[0013] A method for preparing a pearlescent colorful sparkling frit, which is used to prepare the above-mentioned pearlescent colorful sparkling frit, comprises the following steps:

[0014] A. After cerium oxide and perlite are uniformly mixed according to the proportion, water is added to mix to obtain a mixture I; the mixture I is sent to a pelletizer, and after drying, granules I are obtained;

[0015] B. After quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are uniformly mixed according to the proportion, water is added to mix to obtain a mixture II; the mixture II is sent to a ball forming machine, and after drying, granules II are obtained;

[0016] C. After the particles I and II are evenly mixed, a phase separation agent and a flux in a prescribed amount are added, mixed and fired at a high temperature, and then cooled by water quenching and dried to obtain a pearlescent colorful sparkling molten block.

[0017] Furthermore, in step C, the temperature curve of the high temperature firing is:

[0018] It takes 1.5 to 3 hours to rise from room temperature to 500°C;

[0019] It takes 1.5 to 2.5 hours to increase the temperature from 500°C to 1100°C;

[0020] From 1100℃ to 1530℃, it takes 0.2~0.4h;

[0021] 1530℃, keep warm for 0.1~0.2h;

[0022] It takes 0.05 to 0.2 hours to reduce the temperature from 1500°C to 1400°C.

[0023] 1400℃, keep warm for 0.2~0.4h.

[0024] Furthermore, in step C, the temperature curve of the high temperature firing is as follows:

[0025] It takes 2h to rise from room temperature to 500℃;

[0026] It takes 2h to increase the temperature from 500℃ to 1100℃;

[0027] From 1100℃ to 1530℃, it takes 0.3h;

[0028] 1530℃, keep warm for 0.16h;

[0029] It takes 0.1h to reduce the temperature from 1500℃ to 1400℃;

[0030] 1400℃, keep warm for 0.3h.

[0031] The technical solution provided by the present invention may include the following beneficial effects:

[0032] 1. The essence of the pearlescent iridescent frit of the present technical solution is cerium oxide wrapped in fluorphlogopite glass, and the refractive index of the cerium oxide crystal is 2.44, the refractive index of the fluorphlogopite is 1.6, and the refractive index of the glass phase generated by the glass in the frit is 1.54, so that the glaze surface formed by the glaze added with the pearlescent iridescent frit has three crystals with different refractive indices. Since the cerium oxide crystal has a face-centered cubic crystal structure, its crystal plane parallel to the glaze surface has a low interfacial energy, so it shows strong anisotropy during the growth process and has good mirror reflection characteristics for visible light, thus forming a strong mirror reflection. When the incident light shines on the glaze surface formed by the glaze added with the pearlescent iridescent frit, the glaze surface can simultaneously undergo refraction, reflection and interference. And because the fluorphlogopite is translucent and the cerium oxide is white, the glaze surface forms a strong and uniform pearlescent iridescent effect.

[0033] 2. Since the essence of the pearlescent colorful sparkling frit is cerium oxide wrapped in fluorphlogopite glass, that is, the fluorphlogopite is wrapped with cerium oxide with extremely excellent high temperature resistance to form a high temperature resistant protective layer, the high temperature resistance of fluorphlogopite is further ensured, so that the pearlescent colorful sparkling frit can also be used under high temperature firing, thereby increasing its application range. In addition, the cerium oxide in this technical solution is white, and compared with the darker iron oxide, it is not easy to cover the original pattern of the ceramic, thereby ensuring its decorative effect.

[0034] 3. Since the increase in fluorine content will hinder the weakening of hydroxyl groups and lattices at high temperatures, thereby delaying the dehydration and decomposition of fluorophlogopite, that is, the fluorine element in fluorophlogopite plays an important role in stabilizing the lattice structure, significantly improving the thermal stability of fluorophlogopite, and within a certain range, the higher the fluorine content, the greater the degree to which the decomposition temperature of fluorophlogopite can be increased. Therefore, in this technical solution, the amount of potassium fluorosilicate added is limited to 3 to 8 parts to ensure that fluorophlogopite can be formed and its high temperature resistance can be improved at a lower cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a surface microstructure diagram of a ceramic obtained by applying a glaze made from the pearlescent colorful sparkling frit in Example 1 of the present invention to the surface of the ceramic.

[0036] Figure 2 The glaze effect diagram of a ceramic is obtained by applying the glaze made from the pearlescent colorful sparkling frit in Example 1 of the present invention to the surface of the ceramic. DETAILED DESCRIPTION

[0037] The present technical solution provides a pearlescent colorful sparkling frit, which includes the following raw materials, calculated by weight: 8 to 20 parts of perlite, 25 to 35 parts of quartz, 8 to 15 parts of alumina, 10 to 18 parts of fused magnesia, 3 to 8 parts of potassium fluorosilicate, 8 to 15 parts of potassium nitrate, 5 to 10 parts of a phase separator, 5 to 10 parts of cerium oxide and 6 to 16 parts of a flux.

[0038] In order to solve the technical problems in the prior art that the pearlescent fantasy sparkling frit has weak pearlescent fantasy effect, uneven distribution of flash points and is easy to lose its pearlescent fantasy sparkling effect under high-temperature firing, the present technical scheme proposes a pearlescent fantasy sparkling frit, the raw materials of which include perlite, quartz, alumina, fused magnesia, potassium nitrate, phase separation agent, cerium oxide and flux.

[0039] Specifically, the prior art generally uses high-refractive-index oxides (such as iron oxide) to wrap the surface of low-refractive-index mica minerals to form a pearlescent fantasy effect. However, since iron oxide is dark in color and easily turns red, it is easy to cover the original pattern of the ceramic, affecting its decorative effect. In addition, the high-temperature decomposition of mica minerals can easily cause the pearlescent fantasy flash frit to no longer have a pearlescent fantasy effect, so that the pearlescent fantasy flash frit can only be used under low-temperature calcination conditions.

[0040] Therefore, in order to solve the defects in the above-mentioned prior art, the technical scheme uses perlite as a layered structure carrier, uses quartz to increase the silicon element, fused magnesia to provide magnesium, potassium fluorosilicate to provide potassium and fluorine elements, alumina to provide aluminum element and potassium nitrate to provide potassium element, so that quartz, fused magnesia, potassium fluorosilicate, alumina and potassium nitrate react with each other to generate fluorophlogopite with a layered structure, and cerium oxide is wrapped around the outside of the fluorophlogopite to form pearlescent particles of cerium oxide wrapped fluorophlogopite, that is, the essence of the pearlescent fantasy flash frit is cerium oxide wrapped fluorophlogopite glass, and the refractive index of cerium oxide crystals is 2.44, and the refractive index of fluorophlogopite is 1.6. At the same time, the refractive index of the glass phase generated by the glass in the frit is 1.54, so that the glaze surface formed by the glaze added with the pearlescent fantasy flash frit has three crystals with different refractive indices. Since cerium oxide crystals have a face-centered cubic crystal structure, the crystal planes parallel to the glaze surface have low interfacial energy, so they show strong anisotropy during the growth process and have good specular reflection characteristics for visible light, thus forming strong specular reflection. When the incident light irradiates the glaze surface formed by the glaze with the pearlescent fantasy flash frit added, the glaze surface can simultaneously undergo three phenomena: refraction, reflection and interference. Moreover, since fluorphlogopite is translucent and cerium oxide is white, the glaze surface forms a strong and uniform pearl fantasy flash effect. In addition, compared with mica minerals, fluorphlogopite has good high temperature resistance. In addition, since the essence of the pearlescent fantasy flash frit is fluorphlogopite glass wrapped with cerium oxide, that is, fluorphlogopite is wrapped with cerium oxide with extremely excellent high temperature resistance to form a high temperature resistant protective layer, the high temperature resistance of fluorphlogopite is further ensured, so that the pearlescent fantasy flash frit can also be used under high temperature firing, which increases its application range. In addition, the cerium oxide in the present technical solution is white, and compared with the darker iron oxide, it is not easy to cover the original pattern of the ceramic, thereby ensuring its decorative effect.

[0041] It should be noted that fused magnesia is a general term for the products of magnesia raw materials such as magnesia that are molten after high-temperature treatment. Calculated by mass percentage, the chemical composition of fused magnesia includes MgO ≥ 98%, SiO2 ≤ 0.6% and CaO ≤ 1.2%.

[0042] In order to further enhance the pearlescent fantasy sparkle effect of the pearlescent fantasy sparkle frit, the technical solution further adds a phase separation agent to the frit formula. The phase separation agent is easily separated from the glass phase network structure during the heat treatment process, resulting in phase separation. The phase separation can promote the enrichment of cerium oxide in the frit, making it easier for cerium oxide crystals to precipitate and be wrapped around the outside of the layered fluorophlogopite, which not only helps to increase the precipitation amount of pearlescent particles of cerium oxide wrapped in fluorophlogopite, forming a strong and uniform pearlescent fantasy sparkle effect, but also helps to enhance the hardness of the frit.

[0043] Furthermore, since the increase in fluorine content will hinder the weakening of hydroxyl groups and lattices at high temperatures, thereby delaying the dehydration and decomposition of fluorophlogopite, that is, the fluorine element in fluorophlogopite plays an important role in stabilizing the lattice structure, significantly improving the thermal stability of fluorophlogopite, and within a certain range, the higher the fluorine content, the greater the degree to which the decomposition temperature of fluorophlogopite can be increased. Therefore, in the present technical solution, the addition amount of potassium fluorosilicate is limited to 3 to 8 parts to ensure the formation of fluorophlogopite and improve its high temperature resistance at a lower cost.

[0044] In addition, it should be noted that the frit of the present technical solution utilizes the reaction of quartz, alumina and flux to generate a silicate network structure, thereby forming a glass phase, which is beneficial to improving the hardness and wear resistance of the frit. However, due to the high melting points of quartz and alumina, and the large amount of both added, when no flux is added or the amount of flux added is too little, it is easy to cause the frit to fail to be completely calcined during the firing process, affecting the precipitation amount of pearlescent particles of cerium oxide-wrapped fluorphlogopite, and further affecting the pearlescent and colorful sparkling effect of the frit. Therefore, in the present technical solution, the amount of flux added is limited to 6 to 16 parts, which is beneficial to ensure the pearlescent and colorful sparkling effect of the frit.

[0045] It is further described that the mesh number of the cerium oxide is 300-325 meshes, the mesh number of the perlite is 300-325 meshes, and the mesh number of the fused magnesia is 380-400 meshes.

[0046] When the mesh number of cerium oxide is too large, it is easy to increase the roughness of the pearlescent particles of fluorphlogopite wrapped by cerium oxide, thereby affecting the uniformity of the optical illusion effect. When the mesh number of cerium oxide is too small, it is easy to increase the difficulty of grinding, reduce production efficiency, and increase production costs. Therefore, in a preferred embodiment of the present technical solution, the mesh number of cerium oxide is limited to ensure the uniformity of the pearlescent illusion flash effect at a lower cost.

[0047] Furthermore, by limiting the mesh size of perlite and fused magnesia, it is helpful to improve the intensity and uniformity of the pearlescent colorful flash effect.

[0048] It is further described that the flux includes zinc oxide and lithium carbonate, and calculated by mass ratio, the mixing ratio of the zinc oxide and the lithium carbonate is (0.8-1.2):1.

[0049] Both zinc oxide and lithium carbonate have good effects of reducing the firing temperature and promoting sintering. Therefore, in a preferred embodiment of the present technical solution, the flux includes zinc oxide and lithium carbonate, and the mixing ratio of zinc oxide and lithium carbonate is limited to promote high-temperature calcination of the frit, thereby ensuring its pearlescent and colorful flashing effect. In addition, in addition to its fluxing effect, zinc oxide can, on the one hand, act as a nucleus former, reduce the crystallization activation energy and crystallization peak temperature, and is beneficial to the crystallization of cerium oxide, thereby further enhancing the pearlescent and colorful flashing effect; on the other hand, it can also improve the anti-fouling performance.

[0050] It is further specified that the phase separation agent is calcium phosphate.

[0051] Calcium phosphate can produce phosphorus pentoxide when calcined. Due to its high coordination number and strong cationic field, phosphorus pentoxide is easily separated from the glass phase network structure during heat treatment, resulting in phase separation. Phase separation can promote the enrichment of cerium oxide in the frit, making it easier for cerium oxide crystals to precipitate, which is more conducive to improving the pearlescent and colorful flash effect of the frit. In addition, calcium phosphate can also produce calcium oxide when calcined. Calcium oxide can also play a fluxing effect, which is conducive to reducing the calcination temperature of the frit, allowing the frit to be calcined completely, and ensuring the pearlescent and colorful flash effect of the frit.

[0052] It is further explained that, calculated by mass percentage, the chemical composition of the pearlescent colorful sparkling frit includes SiO247-48%, Al2O3 19-22%, Fe2O3 0.2-0.5%, CaO 5-6%, MgO 10-12%, K2O 7-8.5%, ZnO 4.4-4.5%, Na2O 0.02-0.03%, CeO 6-8% and P2O5 3.5-4.5%.

[0053] In another preferred embodiment of the present technical solution, a pearlescent colorful sparkling frit is selected whose chemical composition includes SiO2 47-48%, Al2O3 19-22%, Fe2O3 0.2-0.5%, CaO 5-6%, MgO 10-12%, K2O 7-8.5%, ZnO 4.4-4.5%, Na2O 0.02-0.03%, CeO 6-8% and P2O5 3.5-4.5%, calculated in mass percentage. The SiO2 content is as high as 47-48%, which is a high-silicon frit, which is beneficial to ensure the hardness and wear resistance of the frit.

[0054] Further explanation: calculated by weight, the pearlescent colorful sparkling frit includes the following raw materials: 10 parts of perlite, 32 parts of quartz, 10 parts of alumina, 15 parts of fused magnesia, 5 parts of potassium fluorosilicate, 10 parts of potassium nitrate, 8 parts of phase separation agent, 6 parts of cerium oxide and 9 parts of flux.

[0055] In a preferred embodiment of the present technical solution, the formula of the pearlescent colorful glitter frit is further optimized to achieve the best high temperature resistance of the pearlescent colorful glitter frit and the intensity and uniformity of the pearlescent colorful glitter effect.

[0056] A method for preparing a pearlescent colorful sparkling frit, which is used to prepare the above-mentioned pearlescent colorful sparkling frit, comprises the following steps:

[0057] A. After cerium oxide and perlite are uniformly mixed according to the proportion, water is added to mix to obtain a mixture I; the mixture I is sent to a pelletizer, and after drying, granules I are obtained;

[0058] B. After quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are uniformly mixed according to the proportion, water is added to mix to obtain a mixture II; the mixture II is sent to a ball forming machine, and after drying, granules II are obtained;

[0059] C. After the particles I and II are evenly mixed, a phase separation agent and a flux in a prescribed amount are added, mixed and fired at a high temperature, and then cooled by water quenching and dried to obtain a pearlescent colorful sparkling molten block.

[0060] The technical solution also proposes a method for preparing a pearlescent colorful sparkling frit, which has simple steps and strong operability, and is conducive to ensuring the relevant properties of soft porcelain during the preparation process.

[0061] Specifically, in the technical scheme, cerium oxide and perlite are first mixed evenly according to a ratio, water is added for mixing to obtain mixture I, mixture I is sent to a ball-forming machine, and granules I are obtained after drying, and then quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are mixed evenly according to a ratio, water is added for mixing to obtain mixture II, mixture II is sent to a ball-forming machine, and granules II are obtained after drying, thereby reducing the interface contact area between different raw materials and reducing the mutual penetration between glass phases during the sintering process of the frit, thereby ensuring the precipitation amount of pearlescent particles of cerium oxide-coated fluorphlogopite and ensuring the pearlescent colorful sparkling effect of the frit.

[0062] Further explanation, in step C, the temperature curve of the high temperature firing is:

[0063] It takes 1.5 to 3 hours to rise from room temperature to 500°C;

[0064] It takes 1.5 to 2.5 hours to increase the temperature from 500°C to 1100°C;

[0065] From 1100℃ to 1530℃, it takes 0.2~0.4h;

[0066] 1530℃, keep warm for 0.1~0.2h;

[0067] It takes 0.05 to 0.2 hours to reduce the temperature from 1500°C to 1400°C.

[0068] 1400℃, keep warm for 0.2~0.4h.

[0069] In a preferred embodiment of the present technical solution, the temperature curve of the high-temperature firing of the frit is optimized, which is helpful to ensure the pearlescent colorful sparkling effect of the frit.

[0070] Specifically, the frit is kept at 1530°C for 0.1 to 0.2 h during the high-temperature firing process. If the holding time is too long, the glass content of the frit will increase significantly, destroying the layered structure of perlite and fluorophlogopite, and the pearlescent fantasy sparkle effect will deteriorate. If the holding time is too short, the synthesized amount of fluorophlogopite will be small, and the pearlescent fantasy sparkle effect will also deteriorate.

[0071] More specifically, it takes 0.05 to 0.2 hours for the melt to cool from 1500°C to 1400°C during the high-temperature firing process. If the cooling time is too short, the fluorophlogopite is not completely wrapped, the precipitation amount of pearlescent particles of cerium oxide wrapped fluorophlogopite is reduced, and the pearlescent fantasy flash effect is deteriorated; if the cooling time is too long, the long-term cooling causes the viscosity of the melt to decrease uniformly, which is not conducive to the cerium oxide crystals wrapping the fluorophlogopite, the precipitation amount of pearlescent particles of cerium oxide wrapped fluorophlogopite is also reduced, and the pearlescent fantasy flash effect is also deteriorated.

[0072] Further explanation, in step C, the temperature curve of the high temperature firing is as follows:

[0073] It takes 2h to rise from room temperature to 500℃;

[0074] It takes 2h to increase the temperature from 500℃ to 1100℃;

[0075] From 1100℃ to 1530℃, it takes 0.3h;

[0076] 1530℃, keep warm for 0.16h;

[0077] It takes 0.1h to reduce the temperature from 1500℃ to 1400℃;

[0078] 1400℃, keep warm for 0.3h.

[0079] In a preferred embodiment of the present technical solution, the temperature curve of the high-temperature firing of the frit is further optimized so that the temperature curve of the high-temperature firing is optimized, which is beneficial to ensure that the pearlescent colorful flash effect of the frit is optimal.

[0080] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0081] Example 1

[0082] A. After 6 parts of cerium oxide with a mesh number of 300 and 10 parts of perlite with a mesh number of 325 are mixed evenly, water is added to mix to obtain a mixture I; the mixture I is sent to a pelletizer, and after drying, granules I are obtained;

[0083] B. 32 parts of quartz, 10 parts of alumina, 15 parts of fused magnesia with a mesh size of 400 mesh, 5 parts of potassium fluorosilicate and 10 parts of potassium nitrate are uniformly mixed, and water is added to mix to obtain a mixture II; the mixture II is fed into a ball forming machine, and granules II are obtained after drying;

[0084] C. After mixing granules I and II evenly, add 8 parts of calcium phosphate, 4 parts of zinc oxide and 5 parts of lithium carbonate, mix and sinter at high temperature, quench with water, cool and dry to obtain a pearlescent colorful glittering frit; wherein, the temperature curve of high temperature sintering is as follows: from room temperature to 500°C, it takes 1.5 to 3 hours; from 500°C to 1100°C, it takes 1.5 to 2.5 hours; from 1100°C to 1530°C, it takes 0.2 to 0.4 hours; at 1530°C, keep warm for 0.1 to 0.2 hours; from 1500°C to 1400°C, it takes 0.05 to 0.2 hours; at 1400°C, keep warm for 0.2 to 0.4 hours.

[0085] The pearlescent colorful flashing frit prepared in this embodiment is mixed with kaolin, sodium carboxymethyl cellulose solution, sodium tripolyphosphate and water to form a pearlescent colorful flashing glaze, and the pearlescent colorful flashing glaze is applied to the surface of the ceramic with the base glaze layer to form a ceramic with a pearlescent colorful flashing glaze layer. The surface microstructure of the prepared ceramic is shown in FIG. Figure 1 As shown in the figure, a large number of pearlescent particles of fluorphlogopite wrapped in cerium oxide can be clearly seen distributed in the glass phase of the glaze layer. In addition, the glaze effect is shown in the figure below. Figure 2 As shown, it can be seen that its glaze can present a strong pearlescent fantasy sparkle effect under light conditions, and the sparkle effect is uniform.

[0086] Example 2

[0087] A. After 10 parts of cerium oxide with a mesh number of 325 and 20 parts of perlite with a mesh number of 325 are mixed evenly, water is added to mix to obtain a mixture I; the mixture I is sent to a pelletizer, and after drying, granules I are obtained;

[0088] B. 25 parts of quartz, 8 parts of alumina, 18 parts of fused magnesia with a mesh size of 380, 8 parts of potassium fluorosilicate and 8 parts of potassium nitrate are uniformly mixed, and water is added to mix to obtain a mixture II; the mixture II is fed into a ball forming machine, and granules II are obtained after drying;

[0089] C. After mixing granules I and II evenly, add 10 parts of calcium phosphate, 6 parts of zinc oxide and 5 parts of lithium carbonate, mix and sinter at high temperature, quench with water, cool and dry to obtain a pearlescent colorful glittering frit; wherein, the temperature curve of high temperature sintering is as follows: from room temperature to 500°C, it takes 1.5 to 3 hours; from 500°C to 1100°C, it takes 1.5 to 2.5 hours; from 1100°C to 1530°C, it takes 0.2 to 0.4 hours; at 1530°C, keep warm for 0.1 to 0.2 hours; from 1500°C to 1400°C, it takes 0.05 to 0.2 hours; at 1400°C, keep warm for 0.2 to 0.4 hours.

[0090] Example 3

[0091] A. After uniformly mixing 6 parts of cerium oxide with a mesh number of 325 and 10 parts of perlite with a mesh number of 300, water is added to mix to obtain a mixture I; the mixture I is fed into a pelletizer, and after drying, granules I are obtained;

[0092] B. 30 parts of quartz, 15 parts of alumina, 10 parts of fused magnesia with a mesh size of 400 mesh, 5 parts of potassium fluorosilicate and 15 parts of potassium nitrate are uniformly mixed, and water is added to mix to obtain a mixture II; the mixture II is fed into a ball forming machine, and granules II are obtained after drying;

[0093] C. After mixing granules I and II evenly, add 5 parts of calcium phosphate, 8 parts of zinc oxide and 7 parts of lithium carbonate, mix and sinter at high temperature, quench with water, cool and dry to obtain a pearlescent colorful glittering frit; wherein, the temperature curve of high temperature sintering is as follows: from room temperature to 500°C, it takes 1.5 to 3 hours; from 500°C to 1100°C, it takes 1.5 to 2.5 hours; from 1100°C to 1530°C, it takes 0.2 to 0.4 hours; at 1530°C, keep warm for 0.1 to 0.2 hours; from 1500°C to 1400°C, it takes 0.05 to 0.2 hours; at 1400°C, keep warm for 0.2 to 0.4 hours.

[0094] Comparative Example 1

[0095] The preparation method and raw materials of Comparative Example 1 are the same as those of Example 1, except that cerium oxide is not added to the raw materials in Comparative Example 1.

[0096] Comparative Example 2

[0097] The preparation method and raw materials of Comparative Example 2 are the same as those of Example 1, except that the raw materials in Comparative Example 2 do not contain a phase separation agent, calcium phosphate.

[0098] Comparative Example 3

[0099] The preparation method and raw materials of Comparative Example 3 are the same as those of Example 1, except that quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are not added to the raw materials in Comparative Example 3.

[0100] Comparative Example 4

[0101] The preparation method and raw materials of Comparative Example 4 are the same as those of Example 1, except that mineral mica is used in Comparative Example 4 to replace the quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate that form fluorphlogopite in Example 1, that is, in Comparative Example 4, calculated by weight, the pearlescent colorful sparkling frit includes the following raw materials: 10 parts of perlite, 72 parts of mineral mica, 8 parts of phase separator, 6 parts of cerium oxide and 9 parts of flux.

[0102] The pearlescent colorful flash frits prepared in Examples 1-3 and Comparative Examples 1-4 were mixed with kaolin, sodium carboxymethyl cellulose solution, sodium tripolyphosphate and water to form a pearlescent colorful flash glaze, and the pearlescent colorful flash glaze was applied to the surface of a tile having a base glaze layer to form a tile having a pearlescent colorful flash glaze layer. The tiles were subjected to conventional hardness, glossiness and antifouling grade tests in the field of architectural ceramics. The results are shown in Table 1 below:

[0103] Table 1 Performance test results of glazed tiles of Examples 1-3 and Comparative Examples 1-2

[0104]

[0105] It can be seen from the performance test results in Table 1 that the tiles obtained from the pearlescent iridescent glitter frit of this scheme not only have a strong and uniform pearlescent iridescent effect, but also have good hardness and anti-fouling properties, so that the tiles obtained using the pearlescent iridescent glitter frit have both decorative and practical properties, which is more conducive to meeting the usage needs of consumers.

[0106] In Comparative Example 1, since cerium oxide is not added, pearlescent particles of cerium oxide-coated fluorphlogopite cannot be formed, resulting in a weak pearlescent glitter effect on the glaze of the tile obtained by using the pearlescent glitter frit of Comparative Example 1.

[0107] In Comparative Example 2, since no phase separation agent calcium phosphate is added, it is not conducive to the precipitation of cerium oxide crystals, that is, it is not conducive to the formation of pearlescent particles of cerium oxide-wrapped fluorphlogopite. Although the glaze surface obtained still has a certain pearlescent fantasy effect, compared with the glaze effect of Example 1, the pearlescent fantasy effect of the glaze surface of the tile obtained in Comparative Example 1 is average.

[0108] In Comparative Example 3, since quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are not added, fluorophlogopite cannot be formed, that is, pearlescent particles of fluorphlogopite wrapped with cerium oxide cannot be formed, resulting in weak pearlescent glitter effect of the glaze of the tile obtained using the pearlescent glitter frit of Comparative Example 3.

[0109] Although mineral mica is used in Comparative Example 4 to replace the quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate that form fluorphlogopite in Example 1, the decomposition temperature of mineral mica is between 800 and 900°C, resulting in the decomposition of the pearlescent fantasy frit during the high-temperature firing process, and the cerium oxide-wrapped mineral mica pearlescent particles cannot be formed, resulting in the ceramic tile glaze obtained using the pearlescent fantasy frit of Comparative Example 4 having a weak pearlescent fantasy effect.

[0110] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A pearlescent colorful flash frit, characterized by: Calculated by mass, the raw materials include: 8 to 20 parts of perlite, 25 to 35 parts of quartz, 8 to 15 parts of alumina, 10 to 18 parts of fused magnesia, 3 to 8 parts of potassium fluorosilicate, 8 to 15 parts of potassium nitrate, 5 to 10 parts of phase separation agent, 5 to 10 parts of cerium oxide and 6 to 16 parts of flux.

2. The pearlescent colorful sparkling frit according to claim 1, characterized in that: The mesh number of the cerium oxide is 300-325 meshes, the mesh number of the perlite is 300-325 meshes, and the mesh number of the fused magnesia is 380-400 meshes.

3. The pearlescent colorful sparkling frit according to claim 1, characterized in that: The flux includes zinc oxide and lithium carbonate, and calculated by mass ratio, the mixing ratio of the zinc oxide to the lithium carbonate is (0.8-1.2):

1.

4. The pearlescent colorful sparkling frit according to claim 3, characterized in that: The phase separation agent is calcium phosphate.

5. The pearlescent colorful sparkling frit according to claim 4, characterized in that: Calculated by mass percentage, the chemical composition of the pearlescent colorful sparkling frit includes SiO2 47-48%, Al2O3 19-22%, Fe2O3 0.2-0.5%, CaO 5-6%, MgO 10-12%, K2O 7-8.5%, ZnO 4.4-4.5%, Na2O 0.02-0.03%, CeO 6-8% and P2O5 3.5-4.5%.

6. The pearlescent colorful sparkling frit according to claim 1, characterized in that: Calculated by weight, the pearlescent colorful sparkling frit includes the following raw materials: 10 parts of perlite, 32 parts of quartz, 10 parts of alumina, 15 parts of fused magnesia, 5 parts of potassium fluorosilicate, 10 parts of potassium nitrate, 8 parts of phase separation agent, 6 parts of cerium oxide and 9 parts of flux.

7. A method for preparing a pearlescent colorful glitter frit, characterized in that: The method for preparing the pearlescent colorful sparkling frit according to any one of claims 1 to 6 comprises the following steps: A. After cerium oxide and perlite are uniformly mixed according to the proportion, water is added to mix to obtain a mixture I; the mixture I is sent to a pelletizer, and after drying, granules I are obtained; B. After quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are uniformly mixed according to the proportion, water is added to mix to obtain a mixture II; the mixture II is sent to a ball forming machine, and after drying, granules II are obtained; C. After the particles I and II are evenly mixed, a phase separation agent and a flux in a prescribed amount are added, mixed and fired at a high temperature, and then cooled by water quenching and dried to obtain a pearlescent colorful sparkling molten block.

8. The method for preparing a pearlescent colorful glitter frit according to claim 7, characterized in that: In step C, the temperature curve of the high temperature firing is: It takes 1.5 to 3 hours to rise from room temperature to 500°C; It takes 1.5 to 2.5 hours to increase the temperature from 500°C to 1100°C; From 1100℃ to 1530℃, it takes 0.2~0.4h; 1530℃, keep warm for 0.1~0.2h; It takes 0.05 to 0.2 hours to reduce the temperature from 1500°C to 1400°C. 1400℃, keep warm for 0.2~0.4h.

9. The method for preparing a pearlescent colorful glitter frit according to claim 8, characterized in that: In step C, the temperature curve of the high temperature firing is as follows: It takes 2h to rise from room temperature to 500℃; It takes 2h to increase the temperature from 500℃ to 1100℃; From 1100℃ to 1530℃, it takes 0.3h; 1530℃, keep warm for 0.16h; It takes 0.1h to reduce the temperature from 1500℃ to 1400℃; 1400℃, keep warm for 0.3h.

Citation Information

Patent Citations

  • High-temperature mirror surface flashy fritted glaze and preparation method thereof

    CN102491787A

  • High-temperature bright-red printing glaze, preparation method and preparation method of glazed tile

    CN104130024A

  • Mica-titanium pearlescent glaze for enamel painted porcelain, preparation method of glaze slip and application of mica-titanium pearlescent glaze

    CN108298818A

  • High-strength light egg white glazed porcelain

    CN113149599A