Continuous basalt fiber surface modification method based on sodium hydroxide solution

The treatment of basalt fibers by different concentrations of sodium hydroxide solutions has solved the problem of cumbersomeness and insufficient performance improvement of fiber modification methods in the prior art, significantly improved the fiber strength and interface binding force, and promoted the application of fibers in the field of high performance , achieving economic and environmentally friendly modification effects.

CN118930072APending Publication Date: 2024-11-12XINJIANG TECH INST OF PHYSICS & CHEM CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410995106.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing basalt fiber surface modification methods are cumbersome, harsh, high cost, and lack accuracy and versatility, resulting in the mechanical properties and scalability of the fibers not being optimally improved, especially due to the wetting agent liquid film and hydrophobicity. Modification causes nanoparticles to fall off easily during processing, affecting the mechanical properties of the fiber.

Method used

Continuous basalt fiber surface treatment is carried out using sodium hydroxide solution of different concentrations. By cleaning and coarsing the fiber surface, the wetting and interfacial binding force of the fiber are improved. The fiber strength is significantly improved by 5% w/v sodium hydroxide solution and through The drying and rinsing steps ensure the accuracy of the processing.

Benefits of technology

It significantly improves the mechanical properties of basalt fibers. The strength of a single fiber can reach 1556MPa, which enhances the bonding strength between the fiber and the matrix material, reduces the demand for expensive chemicals, promotes the application of fibers in the field of high performance, and is economical in the method. , environmentally friendly and scalable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930072A_ABST
    Figure CN118930072A_ABST
Patent Text Reader

Abstract

The invention discloses a continuous basalt fiber surface modification method based on a sodium hydroxide solution. According to the method, the surface of the basalt fiber is cleaned and coarsened, and the surface characteristics of the basalt fiber are optimized through sodium hydroxide treatment. And the influence of sodium hydroxide solutions with different concentrations on the diameter, density, mass retention rate and strength of the basalt fiber is systematically analyzed. After the basalt fiber is treated by sodium hydroxide solutions with different concentrations, the diameter of the basalt fiber is 14.16-15.93 [mu] m, the density is 2.22-2.63 g / cm < 3 >, and the maximum strength of a single fiber can reach 1556 MPa. According to the surface treatment method, the roughness of the surface of the fiber is increased, the wettability of the fiber is improved, the basalt fiber and a matrix material have better interface bonding force, and the application of the basalt fiber composite material can be met. The modified basalt fiber plays an important role in the industries of new energy, automobiles, buildings, aerospace and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the fields of fiber engineering and material science, and in particular relates to a continuous basalt fiber surface modification method based on sodium hydroxide solution. Background Art

[0002] Basalt fiber is obtained from naturally melted basalt and marks an important progress in the field of materials. Basalt fiber stands out in the field of advanced materials with its excellent tensile strength, low density, strong corrosion resistance and environmental protection. Basalt fiber is the fourth high-performance fiber after carbon fiber, aramid and ultra-high molecular weight polyethylene fiber, and is one of the four major fibers that my country focuses on developing. The production process of basalt fiber does not contain any additives, which not only ensures environmental sustainability but also improves cost-effectiveness, making it an attractive choice in various industries. Compared with the currently widely used glass fiber, basalt fiber has good mechanical properties, corrosion resistance, low toxicity, flame retardant properties, and green environmental protection, but its potential has not yet been fully realized, especially in high-performance applications. The interface strength between basalt fiber and the matrix material is an important factor affecting the overall performance of the composite material. When basalt fiber is used as a reinforcing material for composite materials, it needs to be surface modified or treated to improve its bonding strength with the matrix material.

[0003] At present, the methods for improving the performance of basalt fiber include a series of chemical, thermal and mechanical treatment methods. CN116903929A discloses a method for modifying basalt fiber, wherein the basalt fiber is pretreated and then dispersed with a dispersant, and then the dispersed basalt fiber is surface treated with a coupling agent to change the dispersion of the fiber in the coupling agent, thereby preparing a basalt fiber reinforced matrix composite material. CN114477797A discloses a method for surface modification of basalt fiber, wherein the basalt fiber treated with a surface deagent is uniformly dispersed in a mixed solution of an aminosilane coupling agent, ethanol and deionized water, and then the basalt fiber treated with deionized water is immersed in a phytic acid aqueous solution, and then the basalt fiber is immersed in an amino-terminated polymer organic solution, and finally cleaned with deionized water, and the modified basalt fiber obtained after drying can be used to improve the interfacial bonding strength of the enhanced epoxy composite material. Although these methods can play a certain role in improvement, there are often some problems, such as cumbersome procedures, harsh conditions, increased costs and environmental problems. Moreover, most methods use acetone soaking, and the problem of the slurry inside the agglomerated fibers not being completely removed is not considered during the acetone soaking. CN112358201A discloses a method for enhancing and modifying basalt fiber sizing agents. With basalt fiber sizing agents as the modification object and the purpose of enhancing the mechanical properties of the original basalt fibers, disilane hydrolyzate or disilane hydrolyzate dispersed with fumed silica is directly introduced into the traditional sizing agent system as an enhanced component. In this method, disilane can be synthesized independently to achieve the regulation of the type of functional groups, the number of functional groups, and the molecular weight in the disilane molecular chain; by adjusting the specific surface area of ​​fumed silica nanoparticles, the use requirements of different sizing agent systems are met, and the effect of enhancing and modifying the basalt fiber sizing agent is achieved. However, due to the presence of the impregnating agent film and the hydrophobic modification of the nanoparticle surface by traditional amphoteric silane, the surface coupling of inorganic fibers and nanoparticles is not conducive, and the interfacial bonding between fibers and particles is weak, which makes the nanoparticles easy to fall off during the later processing, thus seriously affecting the mechanical properties of basalt fibers. In addition, these existing methods lack the precision and versatility required for promotion to industrial applications, resulting in the inability to achieve optimal improvement in the mechanical properties and scalability of basalt fibers.

[0004] To address these challenges, the present invention provides a continuous basalt fiber surface modification method based on sodium hydroxide solution, which optimizes the surface properties of basalt fibers through sodium hydroxide treatment. Sodium hydroxide, known for its alkalinity, is a promising modifier that can be used to change the surface of basalt fibers, thereby affecting their mechanical properties and morphological attributes. However, the specific effects of different concentrations of sodium hydroxide on the properties of basalt fibers have not been fully studied. By methodically studying the effects of different concentrations of sodium hydroxide solutions on the surface treatment of basalt fibers, the present invention not only helps to fundamentally understand basalt fiber modification, but also provides engineers and researchers with a practical framework to fully utilize the properties of basalt fibers, thereby promoting the development of the fiber engineering field and consolidating the position of basalt fibers as a multifunctional high-performance material. Summary of the invention

[0005] The purpose of the present invention is to provide a continuous basalt fiber surface modification method based on sodium hydroxide solution to address the shortcomings of the current existing technology. The method optimizes the surface properties of basalt fibers by cleaning and roughening the surface of basalt fibers and treating them with sodium hydroxide. After being treated with sodium hydroxide solutions of different concentrations, the diameter of the basalt fibers is between 14.16 μm and 15.93 μm, and the density is between 2.22 g / cm 3 -2.63g / cm 3 The maximum strength of a single fiber can reach 1556MPa. This surface treatment method increases the roughness of the fiber surface, improves the wettability of the fiber, and makes the basalt fiber have better interface bonding with the matrix material, so that it can meet the application of basalt fiber composite materials.

[0006] The method for surface modification of continuous basalt fiber based on sodium hydroxide solution of the present invention is carried out according to the following steps:

[0007] a. Mixing sodium hydroxide with purified water, and preparing sodium hydroxide solutions with mass concentrations of 1% w / v, 5% w / v, 10% w / v, 15% w / v, 20% w / v, 25% w / v and 30% w / v respectively by weight / volume;

[0008] b. Soak the basalt fiber in the sodium hydroxide solutions of various concentrations prepared in step a, keep them at room temperature for 24 hours, then take them out, rinse them with deionized water to remove the residual sodium hydroxide, and then dry them at 105° C. for 60 minutes;

[0009] c. The basalt fibers treated in step b were characterized by measuring the changes in their diameter, density, mass retention, tensile strength and surface roughness. The mechanical properties of a single basalt fiber were evaluated using a fiber tensile testing machine. 60 single fibers were tested and the average value was obtained. During the test, the distance between the two chucks was set to 25 mm, and the crosshead speed was fixed to 2 mm / min. The morphology of the basalt fibers before and after alkali treatment was observed using a scanning electron microscope, and the diameter ranged from 14.16 μm to 15.93 μm, and the density ranged from 2.22 g / cm 3 Up to 2.63g / cm 3 , the modified basalt fiber has a single fiber strength of up to 1556MPa.

[0010] The basalt fibers obtained by the method for surface modification of continuous basalt fibers based on sodium hydroxide solution according to the present invention show better quality retention, indicating that durability and resistance are enhanced;

[0011] Compared with the original basalt fiber strength of 1210MPa before treatment, the strength of the treated basalt fiber has increased. Among them, the fiber treated with sodium hydroxide solution with a mass concentration of 5% w / v has the highest strength, which can reach 1556MPa. This is of great significance for improving the performance of basalt fiber in specific applications, reducing the demand for more complex or harmful chemicals, and promoting the application of basalt fiber in high-performance and high-demand fields, especially in new energy, aerospace, automotive, construction and marine industries.

[0012] The advantages of the present invention compared to the prior art are:

[0013] 1. The method of the present invention can significantly improve the mechanical properties of basalt fiber and increase the fiber strength. The strength of basalt fiber treated with 5% w / v sodium hydroxide solution is particularly improved, reaching 1556 MPa. At the same time, the method can accurately control the performance after modification, which has significant advantages over traditional treatment methods.

[0014] 2. Surface treatment can enhance the surface chemical properties of basalt fibers, thereby improving the adhesion of the composite material and making the mechanical properties of the composite material better than those of untreated fibers.

[0015] 3. Compared with other fiber modification technologies that require expensive materials, the method of the present invention utilizes sodium hydroxide, a low-cost and easily available chemical substance, which is more economical and environmentally friendly.

[0016] 4. The treated basalt fiber has a wider application prospect. At the same time, this method does not affect its inherent properties such as thermal stability and corrosion resistance.

[0017] 5. The scalability of this method makes it a feasible solution for large-scale production of basalt fibers, thus promoting its wide application in various industries.

[0018] The present invention discloses a method for surface modification of continuous basalt fiber based on sodium hydroxide solution, which improves the performance of basalt fiber by cleaning and roughening the surface of basalt fiber. The initial basalt fiber has a diameter of 16.02 μm and a density of 2.63 g / cm 3 , strength is 1210MPa. The diameter of the modified basalt fiber ranges from 14.16μm to 15.93μm; the density range is 2.22g / cm 3 -2.63g / cm 3 ; The maximum strength of a single fiber can reach 1556MPa. Modified / high-performance basalt fibers play an important role in industries such as new energy, automobiles, construction, and aerospace. In addition, the present invention not only establishes a simple and efficient modification method in fiber engineering, but also provides an important experimental basis for customizing basalt fiber properties, promoting the development of high-performance basalt fiber composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram of the basalt fiber processing process of the present invention;

[0020] Figure 2 The scanning electron microscope images of the original basalt fiber of the present invention and the basalt fiber treated with NaOH solution of different concentrations, wherein (a) untreated original basalt fiber, (b) basalt fiber treated with 1% w / v NaOH solution, (c) basalt fiber treated with 5% w / v NaOH solution, (d) basalt fiber treated with 10% w / v NaOH solution, (e) basalt fiber treated with 15% w / v NaOH solution, (f) basalt fiber treated with 20% w / v NaOH solution, (g) basalt fiber treated with 25% w / v NaOH solution, and (h) basalt fiber treated with 30% w / v NaOH solution. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below in conjunction with the embodiments, but is not limited to the given embodiments:

[0022] Example 1

[0023] a. Mix sodium hydroxide and purified water to prepare a sodium hydroxide solution having a concentration (weight / volume) of 1% w / v;

[0024] b. Soak the basalt fiber in the sodium hydroxide solution with a concentration of 1% w / v prepared in step a, keep it at room temperature for 24 hours, take it out, rinse it with deionized water to remove the residual sodium hydroxide, and then dry it at a temperature of 105° C. for 60 minutes;

[0025] c. The basalt fiber treated in step b was characterized by measuring the changes in its diameter, density, mass retention rate, tensile strength and surface roughness. The mechanical properties of a single basalt fiber were evaluated using a fiber tensile testing machine. 60 single fibers were tested and the average value was obtained. During the test, the distance between the two chucks was set to 25 mm and the crosshead speed was fixed to 2 mm / min, which met the ASTM C1557-14 standard. The morphology of the basalt fiber before and after alkali treatment was observed using a scanning electron microscope, and the diameter was 15.93 μm and the density was 2.52 g / cm 3 The modified basalt fiber has a single fiber strength of 1319MPa and a quality retention rate of 97.58%.

[0026] Example 2

[0027] a. Mix sodium hydroxide and purified water to prepare a sodium hydroxide solution having a concentration (weight / volume) of 5% w / v;

[0028] b. Soak the basalt fiber in a 5% w / v sodium hydroxide solution prepared in step a, keep it at room temperature for 24 hours, then take it out, rinse it with deionized water to remove the residual sodium hydroxide, and then dry it at 105° C. for 60 minutes;

[0029] c. The basalt fiber treated in step b was characterized by measuring the changes in its diameter, density, mass retention rate, tensile strength and surface roughness. The mechanical properties of a single basalt fiber were evaluated using a fiber tensile testing machine. 60 single fibers were tested and the average value was obtained. During the test, the distance between the two chucks was set to 25 mm and the crosshead speed was fixed to 2 mm / min, which met the ASTM C1557-14 standard. The morphology of the basalt fiber before and after alkali treatment was observed using a scanning electron microscope, and the diameter was 14.16 μm and the density was 2.31 g / cm 3 The modified basalt fiber has a single fiber strength of 1556MPa and a quality retention rate of 98.40%.

[0030] Example 3

[0031] a. Mix sodium hydroxide and purified water to prepare a sodium hydroxide solution having a concentration (weight / volume) of 10% w / v;

[0032] b. Soak the basalt fiber in a 10% w / v sodium hydroxide solution prepared in step a, keep it at room temperature for 24 hours, take it out, rinse it with deionized water to remove the residual sodium hydroxide, and dry it at 105° C. for 60 minutes;

[0033] c. The basalt fiber treated in step b was characterized by measuring the changes in its diameter, density, mass retention rate, tensile strength and surface roughness. The mechanical properties of a single basalt fiber were evaluated using a fiber tensile testing machine. 60 single fibers were tested and the average value was obtained. During the test, the distance between the two chucks was set to 25 mm and the crosshead speed was fixed to 2 mm / min, which met the ASTM C1557-14 standard. The morphology of the basalt fiber before and after alkali treatment was observed using a scanning electron microscope, and the diameter was 15.51 μm and the density was 2.22 g / cm 3 The modified basalt fiber has a single fiber strength of 1370MPa and a quality retention rate of 96.46%.

[0034] Example 4

[0035] a. Mix sodium hydroxide and purified water to prepare a sodium hydroxide solution having a concentration (weight / volume) of 15% w / v;

[0036] b. Soak the basalt fiber in the sodium hydroxide solutions of various concentrations prepared in step a, keep them at room temperature for 24 hours, then take them out, rinse them with deionized water to remove the residual sodium hydroxide, and then dry them at 105° C. for 60 minutes;

[0037] c. The basalt fiber treated in step b was characterized by measuring the changes in its diameter, density, mass retention rate, tensile strength and surface roughness. The mechanical properties of a single basalt fiber were evaluated using a fiber tensile testing machine. 60 single fibers were tested and the average value was obtained. During the test, the distance between the two chucks was set to 25 mm and the crosshead speed was fixed to 2 mm / min, which met the ASTM C1557-14 standard. The morphology of the basalt fiber before and after alkali treatment was observed using a scanning electron microscope, and the diameter was 15.47 μm and the density was 2.38 g / cm 3 The modified basalt fiber has a single fiber strength of 1280MPa and a quality retention rate of 95.26%.

[0038] Example 5

[0039] a. Mix sodium hydroxide and purified water to prepare a sodium hydroxide solution having a concentration (weight / volume) of 20% w / v;

[0040] b. Soak the basalt fiber in a 20% w / v sodium hydroxide solution prepared in step a, keep it at room temperature for 24 hours, then take it out, rinse it with deionized water to remove the residual sodium hydroxide, and then dry it at 105° C. for 60 minutes;

[0041] c. The basalt fiber treated in step b was characterized by measuring the changes in its diameter, density, mass retention rate, tensile strength and surface roughness. The mechanical properties of a single basalt fiber were evaluated using a fiber tensile testing machine. 60 single fibers were tested and the average value was obtained. During the test, the distance between the two chucks was set to 25 mm and the crosshead speed was fixed to 2 mm / min, which met the ASTM C1557-14 standard. The morphology of the basalt fiber before and after alkali treatment was observed using a scanning electron microscope, and the diameter was 14.88 μm and the density was 2.50 g / cm 3 The modified basalt fiber has a single fiber strength of 1343MPa and a quality retention rate of 91.27%.

[0042] Example 6

[0043] a. Mix sodium hydroxide and purified water to prepare a sodium hydroxide solution having a concentration (weight / volume) of 25% w / v;

[0044] b. Soak the basalt fiber in a 25% w / v sodium hydroxide solution prepared in step a, keep it at room temperature for 24 hours, then take it out, rinse it with deionized water to remove the residual sodium hydroxide, and then dry it at 105° C. for 60 minutes;

[0045] c. The basalt fiber treated in step b was characterized by measuring the changes in its diameter, density, mass retention rate, tensile strength and surface roughness. The mechanical properties of a single basalt fiber were evaluated using a fiber tensile testing machine. 60 single fibers were tested and the average value was obtained. During the test, the distance between the two chucks was set to 25 mm and the crosshead speed was fixed to 2 mm / min, which met the ASTM C1557-14 standard. The morphology of the basalt fiber before and after alkali treatment was observed using a scanning electron microscope, and the diameter was 15.85 μm and the density was 2.49 g / cm 3 The modified basalt fiber has a single fiber strength of 1136MPa and a quality retention rate of 88.64%.

[0046] Example 7

[0047] a. Mix sodium hydroxide and purified water to prepare sodium hydroxide solutions with a concentration (weight / volume) of 30% w / v;

[0048] b. Soak the basalt fiber in a 30% w / v sodium hydroxide solution prepared in step a, keep it at room temperature for 24 hours, then take it out, rinse it with deionized water to remove the residual sodium hydroxide, and then dry it at 105° C. for 60 minutes;

[0049] c. The basalt fiber treated in step b was characterized by measuring the changes in its diameter, density, mass retention rate, tensile strength and surface roughness. The mechanical properties of a single basalt fiber were evaluated using a fiber tensile testing machine. 60 single fibers were tested and the average value was obtained. During the test, the distance between the two chucks was set to 25 mm and the crosshead speed was fixed to 2 mm / min, which met the ASTM C1557-14 standard. The morphology of the basalt fiber before and after alkali treatment was observed using a scanning electron microscope, and the diameter was 15.39 μm and the density was 2.51 g / cm 3 The modified basalt fiber has a single fiber strength of 1203MPa and a quality retention rate of 84.25%.

[0050] Example 8

[0051] The present invention discloses a method for surface modification of continuous basalt fiber based on sodium hydroxide solution. The effectiveness of the method in enhancing the mechanical properties of the fiber is shown in Table 1. The effects of different concentrations of sodium hydroxide solution on the surface treatment of basalt fiber are systematically evaluated:

[0052] Table 1 Comparative data of basalt fiber diameter and density

[0053]

[0054] Table 1 shows the changes in the diameter and density of basalt fibers after treatment. Compared with before treatment, both the diameter and density of basalt fibers decreased, indicating that after sodium hydroxide treatment, the physical structure of basalt fibers has undergone beneficial changes, thereby improving its applicability in specific applications. In addition, Table 1 also provides the mass retention rate and strength data of single basalt fibers after treatment. Despite the chemical reaction during the treatment process, a high quality retention rate is maintained, that is, the quality loss in this process is minimal. It is worth noting that the strength of a single fiber is most significantly improved after treatment with a sodium hydroxide solution with a concentration of 5% w / v. This increase in strength is particularly important for industries that require high-performance materials.

Claims

1. A method for surface modification of continuous basalt fiber based on sodium hydroxide solution, It is characterized in that Follow these steps: a. Mix sodium hydroxide and purified water to prepare sodium hydroxide solutions with mass concentrations of 1% w / v, 5% w / v, 10% w / v, 15% w / v, 20% w / v, 25% w / v and 30% w / v, respectively, by weight / volume; b. Soak the basalt fiber in the sodium hydroxide solutions of various concentrations prepared in step a, keep them at room temperature for 24 hours, take them out, rinse them with deionized water to remove the residual sodium hydroxide, and then dry them at 105° C. for 60 minutes; c. The basalt fibers treated in step b were characterized by measuring the changes in their diameter, density, mass retention, tensile strength and surface roughness. The mechanical properties of a single basalt fiber were evaluated using a fiber tensile testing machine. 60 single fibers were tested and the average value was obtained. During the test, the distance between the two chucks was set to 25 mm, and the crosshead speed was fixed to 2 mm / min. The morphology of the basalt fibers before and after alkali treatment was observed using a scanning electron microscope, and the diameter range was 14.16-15.93 μm and the density range was 2.22-2.63 g / cm 3 , the modified basalt fiber has a single fiber strength of up to 1556 MPa.

Citation Information

Patent Citations

  • Basalt fiber surface modification method

    CN114477797A

  • Method for grafting and modifying basalt fibers by using carboxylated carbon nanotubes

    CN117185694A

  • Method for improving interface bonding and wear resistance of basalt fiber composite material

    CN118290821A

Cited By

  • Inorganic high-strength artificial quartz stone and preparation method thereof

    CN119707402A