Application of nanofluid admixture in neat paste
By using nanofluid external dopants in cement substrates, combining surfactant and graphene, the problems of low dispersion and high cost in cement substrates are solved, and retarding, reducing hydration heat and optimization are achieved The effect of pore structure is suitable for large-scale applications.
Patent Information
- Application Number
- CN202411011210.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The application of nanomaterials in cement substrates has problems such as low dispersion, high cost and difficulty in scale.
Using nanofluid external dopants, the modified cement slurry is prepared by adding surfactants such as polyvinyl alcohol and carboxymethyl cellulose, combined with graphene, to improve the dispersion and cost-effectiveness of the nanofluid, and through shear peeling and emulsification Dispersion technology achieves uniform dispersion of graphene.
It realizes the retarding of cement, reduces hydration heat, optimizes the pore structure, improves dispersion and cost-effectiveness, and facilitates large-scale application.
Smart Images

Figure CN118930113A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical materials, and in particular relates to the application of a nanofluid admixture in clean slurry. Background Art
[0002] The particle size of nanomaterials is usually between 0.1 and 100 nm, and they have small size effects, quantum effects, and nucleation effects. The larger specific surface area of nanomaterials is conducive to the hydration reaction of cement, so that the hydration products are regularly wrapped around the nanomaterials, promoting the generation of more compact hydration products. Therefore, nanomaterials provide a new direction for the preparation and application of high-performance cement-based composites. However, there are technical bottlenecks in the application of nanomaterials in cement substrates (neat slurry), such as low dispersibility, high cost, and difficulty in scale. Summary of the invention
[0003] The purpose of the present invention is to provide an application of a nanofluid admixture in mortar, which solves the problems of technical bottlenecks, low dispersibility, high cost and difficulty in scalability in the application of existing nanomaterials in mortar.
[0004] In order to achieve the above object, the technical solution of the present invention is implemented as follows: a nanofluid admixture is used in the clean slurry.
[0005] In some embodiments, the specific method of the application is: adding the nanofluid admixture into cement paste to obtain modified cement paste.
[0006] In some embodiments, the nanofluid admixture contains a surfactant, and the surfactant is at least one of polyvinyl alcohol and sodium carboxymethyl cellulose.
[0007] In some embodiments, the mass fraction of graphene in the nanofluid admixture is 0.02% to 0.12%; the mass fraction of the nanofluid admixture in the modified pure slurry is 0.05% to 0.08%.
[0008] Compared with the prior art, the nanofluid admixture in the present invention can slow down the setting of the pure slurry, reduce the hydration heat and optimize the pore structure. In addition, it has high dispersibility, low cost and is easy to apply on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 The effect of different graphene dosages on the setting time of PVA-GNAs modified cement in the embodiment of the present invention;
[0010] Figure 2 The effect of different graphene dosages on the setting time of CMC-GNAs modified cement in the embodiment of the present invention;
[0011] Figure 3: is the hydration heat release rate curve of PVA-GNAs modified cement paste at different graphene dosages in the embodiment of the present invention;
[0012] Figure 4 : is the hydration heat release rate curve of CMC-GNAs modified cement paste at different graphene dosages in the embodiment of the present invention;
[0013] Figure 5 : The cumulative hydration exothermic curve of PVA-GNAs modified cement paste at different graphene dosages in the embodiment of the present invention;
[0014] Figure 6 This is the cumulative hydration exothermic curve of CMC-GNAs modified cement paste at different graphene dosages in the embodiment of the present invention. DETAILED DESCRIPTION
[0015] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0016] The PVA in the present invention is polyvinyl alcohol, the CMC is carboxymethyl cellulose, and the graphene nanofluid admixture is GNAs.
[0017] Example 1
[0018] The nanofluid admixture provided in this embodiment 1 is obtained by the following steps:
[0019] Step 1: Pour 5 g of PVA powder and 500 mL of deionized water into a beaker and seal it tightly with a film. Then, heat and stir it continuously for 24 hours using a constant temperature magnetic stirrer set at 80 ° C to ensure that the powder is completely dissolved to form a uniform 10 g / L PVA solution.
[0020] Step 2, shear exfoliation: adding a certain amount of graphite powder to the solution in step 1, and performing shear exfoliation by high-speed stirring. In this step, shear force is generated by the high-speed rotation of the stirrer, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder;
[0021] Step 3, emulsification and dispersion: Then, the mixed solution is emulsified and dispersed using a centrifuge with a rotation speed of 6000 rpm to further improve the uniform dispersion of the graphene nanosheets;
[0022] Step 4: Centrifugal separation: The mixed solution is centrifuged at a high speed of 10,000 rpm to effectively separate the fully exfoliated graphene nanosheets from the incompletely exfoliated graphene sheets, and the supernatant after centrifugation is collected to obtain the desired GNAs;
[0023] The graphene nanofluid admixture is used instead of water and mixed and stirred with cement according to the designed mix ratio to obtain a modified pure slurry. The mass fraction of the graphene nanofluid admixture in the modified pure slurry obtained in Example 1 is 0.06%; the mass fraction of graphene in the graphene nanofluid admixture is 0.05%.
[0024] Example 2
[0025] The nanofluid admixture provided in this embodiment 2 is obtained by the following steps:
[0026] Step 1: Pour 5 g of PVA powder and 500 mL of deionized water into a beaker and seal it tightly with a film. Then, heat and stir it continuously for 24 hours using a constant temperature magnetic stirrer set at 80 ° C to ensure that the powder is completely dissolved to form a uniform 10 g / L PVA solution.
[0027] Step 2, shear exfoliation: adding a certain amount of graphite powder to the solution in step 1, and performing shear exfoliation by high-speed stirring. In this step, shear force is generated by the high-speed rotation of the stirrer, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder;
[0028] Step 3, emulsification and dispersion: Then, the mixed solution is emulsified and dispersed using a centrifuge with a rotation speed of 6000 rpm to further improve the uniform dispersion of the graphene nanosheets;
[0029] Step 4: Centrifugal separation: The mixed solution is centrifuged at a high speed of 10,000 rpm to effectively separate the fully exfoliated graphene nanosheets from the incompletely exfoliated graphene sheets, and the supernatant after centrifugation is collected to obtain the desired GNAs;
[0030] The graphene nanofluid admixture is used instead of water and mixed and stirred with cement according to the designed mix ratio to obtain a modified pure slurry. The mass fraction of the graphene nanofluid admixture in the modified pure slurry obtained in Example 2 is 0.06%; the mass fraction of graphene in the graphene nanofluid admixture is 0.1%.
[0031] Example 3
[0032] The nanofluid admixture provided in this embodiment 3 is obtained by the following steps:
[0033] Step 1: Pour 5 g of PVA powder and 500 mL of deionized water into a beaker and seal it tightly with a film. Then, heat and stir it continuously for 24 hours using a constant temperature magnetic stirrer set at 80 ° C to ensure that the powder is completely dissolved to form a uniform 10 g / L PVA solution.
[0034] Step 2, shear exfoliation: adding a certain amount of graphite powder to the solution in step 1, and performing shear exfoliation by high-speed stirring. In this step, shear force is generated by the high-speed rotation of the stirrer, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder;
[0035] Step 3, emulsification and dispersion: Then, the mixed solution is emulsified and dispersed using a centrifuge with a rotation speed of 6000 rpm to further improve the uniform dispersion of the graphene nanosheets;
[0036] Step 4: Centrifugal separation: The mixed solution is centrifuged at a high speed of 10,000 rpm to effectively separate the fully exfoliated graphene nanosheets from the incompletely exfoliated graphene sheets, and the supernatant after centrifugation is collected to obtain the desired GNAs;
[0037] The graphene nanofluid admixture is used instead of water and mixed and stirred with cement according to the designed mix ratio to obtain a modified pure slurry. The mass fraction of the graphene nanofluid admixture in the modified pure slurry obtained in Example 3 is 0.06%; the mass fraction of graphene in the graphene nanofluid admixture is 0.15%.
[0038] Example 4
[0039] The nanofluid admixture provided in this embodiment 1 is obtained by the following steps:
[0040] Step 1: Pour 5 g of PVA powder and 500 mL of deionized water into a beaker and seal it tightly with a film. Then, heat and stir it continuously for 24 hours using a constant temperature magnetic stirrer set at 80 ° C to ensure that the powder is completely dissolved to form a uniform 10 g / L PVA solution.
[0041] Step 2, shear exfoliation: adding a certain amount of graphite powder to the solution in step 1, and performing shear exfoliation by high-speed stirring. In this step, shear force is generated by the high-speed rotation of the stirrer, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder;
[0042] Step 3, emulsification and dispersion: Then, the mixed solution is emulsified and dispersed using a centrifuge with a rotation speed of 6000 rpm to further improve the uniform dispersion of the graphene nanosheets;
[0043] Step 4: Centrifugal separation: The mixed solution is centrifuged at a high speed of 10,000 rpm to effectively separate the fully exfoliated graphene nanosheets from the incompletely exfoliated graphene sheets, and the supernatant after centrifugation is collected to obtain the desired GNAs;
[0044] The graphene nanofluid admixture is used instead of water and mixed and stirred with cement according to the designed mix ratio to obtain a modified pure slurry. The mass fraction of the graphene nanofluid admixture in the modified pure slurry obtained in Example 4 is 0.06%; the mass fraction of graphene in the graphene nanofluid admixture is 0.2%.
[0045] Example 5
[0046] The nanofluid admixture provided in this embodiment 5 is obtained by the following steps:
[0047] Step 1: Pour 5g of CMC powder and 500mL of deionized water into a beaker and seal it tightly with a film. Then, heat and stir it continuously for 24h using a constant temperature magnetic stirrer set at 80°C to ensure that the powder is completely dissolved to form a uniform 10g / L CMC solution.
[0048] Step 2, shear exfoliation: adding a certain amount of graphite powder to the solution in step 1, and performing shear exfoliation by high-speed stirring. In this step, shear force is generated by the high-speed rotation of the stirrer, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder;
[0049] Step 3, emulsification and dispersion: Then, the mixed solution is emulsified and dispersed using a centrifuge with a rotation speed of 6000 rpm to further improve the uniform dispersion of the graphene nanosheets;
[0050] Step 4: Centrifugal separation: centrifuge the mixed solution at a high speed of 10,000 rpm to effectively separate the fully exfoliated graphene nanosheets from the incompletely exfoliated graphene sheets; collect the supernatant after centrifugation to obtain the desired GNAs;
[0051] The graphene nanofluid admixture is used instead of water and mixed and stirred with cement according to the designed mix ratio to obtain a modified pure slurry. The mass fraction of the graphene nanofluid admixture in the modified pure slurry obtained in Example 5 is 0.06%; the mass fraction of graphene in the graphene nanofluid admixture is 0.02%.
[0052] Example 6
[0053] The nanofluid admixture provided in this embodiment 5 is obtained by the following steps:
[0054] Step 1: Pour 5g of CMC powder and 500mL of deionized water into a beaker and seal it tightly with a film. Then, heat and stir it continuously for 24h using a constant temperature magnetic stirrer set at 80°C to ensure that the powder is completely dissolved to form a uniform 10g / L CMC solution.
[0055] Step 2, shear exfoliation: adding a certain amount of graphite powder to the solution in step 1, and performing shear exfoliation by high-speed stirring. In this step, shear force is generated by the high-speed rotation of the stirrer, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder;
[0056] Step 3, emulsification and dispersion: Then, the mixed solution is emulsified and dispersed using a centrifuge with a rotation speed of 6000 rpm to further improve the uniform dispersion of the graphene nanosheets;
[0057] Step 4: Centrifugal separation: centrifuge the mixed solution at a high speed of 10,000 rpm to effectively separate the fully exfoliated graphene nanosheets from the incompletely exfoliated graphene sheets; collect the supernatant after centrifugation to obtain the desired GNAs;
[0058] The graphene nanofluid admixture is used instead of water and mixed and stirred with cement according to the designed mix ratio to obtain a modified pure slurry. The mass fraction of the graphene nanofluid admixture in the modified pure slurry obtained in Example 6 is 0.06%; the mass fraction of graphene in the graphene nanofluid admixture is 0.04%.
[0059] Example 7
[0060] The nanofluid admixture provided in this embodiment 7 is obtained by the following steps:
[0061] Step 1: Pour 5g of CMC powder and 500mL of deionized water into a beaker and seal it tightly with a film. Then, heat and stir it continuously for 24h using a constant temperature magnetic stirrer set at 80°C to ensure that the powder is completely dissolved to form a uniform 10g / L CMC solution.
[0062] Step 2, shear exfoliation: adding a certain amount of graphite powder to the solution in step 1, and performing shear exfoliation by high-speed stirring. In this step, shear force is generated by the high-speed rotation of the stirrer, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder;
[0063] Step 3, emulsification and dispersion: Then, the mixed solution is emulsified and dispersed using a centrifuge with a rotation speed of 6000 rpm to further improve the uniform dispersion of the graphene nanosheets;
[0064] Step 4: Centrifugal separation: centrifuge the mixed solution at a high speed of 10,000 rpm to effectively separate the fully exfoliated graphene nanosheets from the incompletely exfoliated graphene sheets; collect the supernatant after centrifugation to obtain the desired GNAs;
[0065] The graphene nanofluid admixture is used instead of water and mixed and stirred with cement according to the designed mix ratio to obtain a modified pure slurry. The mass fraction of the graphene nanofluid admixture in the modified pure slurry obtained in Example 7 is 0.06%; the mass fraction of graphene in the graphene nanofluid admixture is 0.06%.
[0066] Example 8
[0067] The nanofluid admixture provided in this embodiment 8 is obtained by the following steps:
[0068] Step 1: Pour 5g of CMC powder and 500mL of deionized water into a beaker and seal it tightly with a film. Then, heat and stir it continuously for 24h using a constant temperature magnetic stirrer set at 80°C to ensure that the powder is completely dissolved to form a uniform 10g / L CMC solution.
[0069] Step 2, shear exfoliation: adding a certain amount of graphite powder to the solution in step 1, and performing shear exfoliation by high-speed stirring. In this step, shear force is generated by the high-speed rotation of the stirrer, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder;
[0070] Step 3, emulsification and dispersion: Then, the mixed solution is emulsified and dispersed using a centrifuge with a rotation speed of 6000 rpm to further improve the uniform dispersion of the graphene nanosheets;
[0071] Step 4: Centrifugal separation: centrifuge the mixed solution at a high speed of 10,000 rpm to effectively separate the fully exfoliated graphene nanosheets from the incompletely exfoliated graphene sheets; collect the supernatant after centrifugation to obtain the desired GNAs;
[0072] The graphene nanofluid admixture is used instead of water and mixed and stirred with cement according to the designed mix ratio to obtain a modified pure slurry. The mass fraction of the graphene nanofluid admixture in the modified pure slurry obtained in Example 8 is 0.06%; the mass fraction of graphene in the graphene nanofluid admixture is 0.08%.
[0073] Example 9
[0074] The nanofluid admixture provided in this embodiment 9 is obtained by the following steps:
[0075] Step 1: Pour 5g of CMC powder and 500mL of deionized water into a beaker and seal it tightly with a film. Then, heat and stir it continuously for 24h using a constant temperature magnetic stirrer set at 80°C to ensure that the powder is completely dissolved to form a uniform 10g / L CMC solution.
[0076] Step 2, shear exfoliation: adding a certain amount of graphite powder to the solution in step 1, and performing shear exfoliation by high-speed stirring. In this step, shear force is generated by the high-speed rotation of the stirrer, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder;
[0077] Step 3, emulsification and dispersion: Then, the mixed solution is emulsified and dispersed using a centrifuge with a rotation speed of 6000 rpm to further improve the uniform dispersion of the graphene nanosheets;
[0078] Step 4: Centrifugal separation: centrifuge the mixed solution at a high speed of 10,000 rpm to effectively separate the fully exfoliated graphene nanosheets from the incompletely exfoliated graphene sheets; collect the supernatant after centrifugation to obtain the desired GNAs;
[0079] The graphene nanofluid admixture is used instead of water and mixed and stirred with cement according to the designed mix ratio to obtain a modified pure slurry. The mass fraction of the graphene nanofluid admixture in the modified pure slurry obtained in Example 9 is 0.06%; the mass fraction of graphene in the graphene nanofluid admixture is 0.1%.
[0080] The following is an example of applying the above graphene nanofluid admixture to the clean slurry.
[0081] The graphene nanofluid admixtures obtained in Examples 1 to 4 were added to cement pastes to obtain four modified cement pastes, and the setting time of the four modified cement pastes was tested. Figure 1 shown.
[0082] By analyzing Figure 1 It can be seen that polyvinyl alcohol (PVA) plays a key retarding role in PVA-GNAs modified cement matrix (neat paste). PVA not only increases the viscosity of the cement paste by interacting with the surface of cement particles, but also "captures" water molecules and cement particles by forming a network structure, thereby slowing down the rate of the hydration reaction. This retarding effect is due to the fact that the PVA molecular chain can form a physical barrier in the cement paste that hinders the free movement and reaction of water molecules and cement particles, resulting in a prolonged setting time. The addition of graphene brings about a nucleation effect. Due to its extremely high specific surface area, it can provide a large number of nucleation sites, which theoretically helps to accelerate the occurrence of hydration reactions. The high-energy sites on the graphene surface adsorb water molecules, providing an optimized local environment for the formation of hydration products, which theoretically should be able to promote the acceleration of the setting process.
[0083] However, in PVA-GNAs modified cement, the retarding effect of polyvinyl alcohol and the nucleation effect of graphene form a complex competitive relationship. On the one hand, the retarding effect of PVA slows down the hydration reaction rate and prolongs the setting time; on the other hand, the nucleation effect of graphene attempts to accelerate this process; with the increase of graphene content, this competitive relationship leads to the extension of initial and final setting time, especially the extension of final setting time is more significant. This phenomenon occurs mainly because, although graphene may promote the occurrence of hydration reaction in the early stage, as the reaction proceeds, the retarding effect of PVA gradually dominates, especially in the later stage of hydration reaction, the influence of PVA becomes more obvious, resulting in a significant extension of final setting time.
[0084] The graphene nanofluid admixtures obtained in Examples 5 to 9 were added to cement pastes to obtain five modified cement pastes, and the setting time of the five modified cement pastes was tested. Figure 2 shown.
[0085] By analyzing Figure 2 It can be seen that sodium carboxymethyl cellulose (CMC) plays a retarding role in CMC-GNAs modified cement. This is mainly because CMC, as a surfactant, can form an adsorption film on the surface of cement particles. This film not only increases the viscosity of the cement paste, but also reduces the rate of hydration reaction. CMC molecules reduce the direct contact between water molecules and cement particles through adsorption on the surface of cement particles, thereby slowing down the hydration process.
[0086] Similarly, in CMC-GNAs modified cement, the retarding effect of CMC competes with the nucleation effect of graphene. Although graphene has the potential to promote hydration, the presence of CMC significantly slows down the overall hydration rate, resulting in an overall extension of the setting time; this competitive relationship makes the increments of the initial and final setting times almost the same, 360 min and 375 min, respectively, indicating that the effects of the two materials maintain a consistent influence throughout the hydration process.
[0087] In summary, the different strengths of the competitive relationship between graphene and surfactants in PVA-GNAs and CMC-GNAs modified cement matrices (paste) can be partly attributed to the fact that the graphene concentration in GNAs made from CMC is higher than that in GNAs made from PVA at the same ratio. Specifically, the graphene concentration in GNAs made from CMC is about 20 g / L, while the graphene concentration in GNAs made from PVA is only about 4.5 g / L. This means that under the condition of the same graphene dosage, the concentration of PVA is actually higher, so the effect of PVA in modified cement is relatively more significant.
[0088] The graphene nanofluid admixtures obtained in Examples 1 to 4 were added to cement pastes to obtain four modified cement pastes, and the hydration heat release rates of the four modified cement pastes were tested. Figure 3 As shown; the graphene nanofluid admixtures obtained in Examples 5 to 9 were added to cement pastes to obtain five modified cement pastes, and the hydration heat release rates of the five modified cement pastes were tested. The specific test results are as follows: Figure 4 shown.
[0089] By analyzing Figure 3 It can be seen that in the accelerated period of hydration (III), with the increase of graphene content, the exothermic peak intensity of silicate decreased and the time of peak appearance was delayed. This phenomenon indicates that PVA-GNAs may inhibit the hydration reaction of calcium trisilicate (C3S) to a certain extent, which is one of the main reactions of cement setting and hardening. Since the hydration rate of C3S is slowed down, the heat released by the hydration reaction is reduced during the initial and accelerated period of cement setting, resulting in a decrease and delay in the heat flow peak. The high specific surface area and adsorption characteristics of GNAs may lead to a weakened interaction between water molecules and cement particles, thereby reducing the reaction rate. This may be due to the physical barrier formed by PVA-GNAs on the surface of cement particles, as well as their possible chemical interactions, which may lead to a slowdown in the dissolution of C3S and the subsequent generation of CSH and CH.
[0090] In the deceleration period (IV), as the graphene doping amount increases, the peak intensity of the sulfate depletion peak decreases and the time of peak appearance is also delayed. This indicates that the incorporation of PVA-GNAs also delays the solute reaction of C3A to form ettringite, and PVA-GNAs may affect the interaction between C3A and sulfate. The main reformation of ettringite increased significantly, while the rapid formation of monosulfate was completed in a shorter time. This may be because the nucleation effect of graphene may play a more complex role in the sulfate hydration reaction. Since graphene may provide additional nucleation sites, this may promote the formation of early ettringite, but with the increase in doping, the blocking effect of acetate in PVA may become more significant, which will affect the availability of water and sulfate, thereby reducing the intensity of the sulfate depletion peak in the later stage. It happens that this is also the period when the effect of different graphene doping amounts on the hydration heat is most obvious. Therefore, it can be inferred that the effect of GNAs on hydration during this period mainly affects the formation of two hydration products, ettringite and monosulfate. By analyzing Figure 4It can be seen that, whether it is PVA-GNAs or CMC-GNAs, with the increase of graphene content, both materials can delay the appearance time of the first and second exothermic peaks in cement paste and reduce the intensity of the exothermic peaks. This shows that the addition of GNAs has a significant effect on the cement hydration kinetics, delays the hydration reaction, and reduces the rate of heat release.
[0091] The difference is that during the PVA-GNAs modification process, although the intensity of the second exothermic peak decreases with the increase of graphene doping, its intensity is still higher than that of the blank group without GNAs. This reflects the competitive relationship between PVA and graphene, that is, there is a dynamic balance between the retarding effect of PVA and the nucleation sites provided by graphene. At certain doping amounts, although PVA reduces the hydration rate, the high specific surface area and nucleation ability of graphene are still sufficient to maintain a high exothermic intensity. The CMC-GNAs component shows a different behavior from PVA-GNAs. The exothermic peak of CMC-GNAs is lower than that of the blank group at all doping amounts, and with the increase of graphene doping, the rate and intensity of hydration exothermicity are fully delayed. This may be because CMC, as a surfactant, provides stronger adsorption capacity and a more stable hydration reaction barrier compared with PVA. CMC-GNAs do not show a significant competitive relationship with graphene, but show a more synergistic effect between graphene and CMC, which makes CMC-GNAs more ideal in controlling hydration heat.
[0092] This study speculates that this synergistic effect may be due to the following two reactions: On the one hand, the carboxyl groups in CMC can increase the viscosity of the cement paste by adsorbing on the surface of cement particles, thereby physically hindering the hydration reaction. On the other hand, the carboxyl groups of CMC may form complexes with calcium ions. In fact, the formation of the complex may reduce the concentration of free calcium ions, thereby affecting the hydration rate, but will not significantly change the pH value.
[0093] The graphene nanofluid admixtures obtained in Examples 1 to 4 were added to cement pastes to obtain four modified cement pastes, and the cumulative hydration heat release rates of the four modified cement pastes were tested. Figure 5 As shown; the graphene nanofluid admixtures obtained in Examples 5 to 9 were added to cement pastes to obtain five modified cement pastes, and the cumulative hydration heat release rates of the five modified cement pastes were tested. The specific test results are as follows: Figure 6 shown.
[0094] By analyzing Figure 5It can be seen that the cumulative heat release curve shows that the total heat release of cement paste after adding PVA-GNAs is generally less than that of the blank group in the initial hydration period. This is because the addition of PVA-GNAs slows down the initial rate of cement hydration reaction, especially affecting the hydration reaction of C3S and C3A, which are the main sources of cement hydration heat.
[0095] When observing the final cumulative heat release, it can be seen that the total heat release decreases significantly with the increase in the PVA-GNAs dosage. This may be because higher dosages of PVA-GNAs enhance their effects on the hydration reaction, especially in the later stages of hydration. Because higher dosages of GNAs may not only affect the dissolution of C3S in the early stages of hydration, but also affect the hydration of C3A and its reaction with sulfate in the middle and late stages of hydration, thereby reducing the heat release during the entire hydration process. In addition, the analysis shows that PVA and graphene in GNAs have a competitive relationship in their effects on the heat of cement hydration. PVA may be mainly responsible for slowing down the hydration rate, while graphene may promote the hydration process to some extent, especially by providing nucleation sites. With the increase in dosage, these two effects may have been enhanced or antagonized to varying degrees, resulting in a complex nonlinear relationship. This further suggests that the composition and dosage of GNAs need to be designed more accurately through modeling.
[0096] In conclusion, the incorporation of GNAs has a significant effect on the cumulative heat release of cement hydration heat, which demonstrates the potential of GNAs as cement admixtures in regulating cement hydration heat and optimizing cement paste properties. However, in order to maximize its effect, further research and optimization of the formulation and incorporation amount of GNAs are needed to effectively control the development of cement hydration heat without sacrificing cement strength and durability.
[0097] By analyzing Figure 6 It can be seen that with the increase of CMC-GNAs dosage, the rising trend of the total hydration heat release is relatively slowed down. This shows that CMC-GNAs effectively delays the cement hydration reaction, especially at higher dosages, the rate of increase of heat release is low, showing its potential in controlling the development of hydration heat. Specifically, compared with the blank sample without GNAs, CMC-GNAs also show the ability to reduce the rate of hydration heat release even at the lowest dosage (0.07wt%). This delaying effect increases with the increase of dosage, especially at high dosages such as 0.64wt% and 0.92wt%. The slope of the cumulative heat release curve in the high dosage sample is significantly lower than that of the blank sample, which shows that CMC-GNAs plays a key role in slowing down the early and mid-stage hydration reaction. It should be noted that the hydration heat test time is 72 hours. Therefore, although the curve in the figure shows the heat release trend within 72 hours, the actual total amount of cement hydration heat release may still increase after the test time.
[0098] The addition of CMC-GNAs showed a significant effect in reducing the total amount of cement hydration heat in the 72-hour hydration heat test, which not only slowed down the cement hydration reaction rate, but also helped to reduce the internal stress and crack risk caused by hydration heat.
[0099] In summary, although both PVA-GNAs and CMC-GNAs can effectively control cement hydration exotherm, CMC-GNAs provide a more balanced and comprehensive control effect. With the increase of graphene content, CMC-GNAs can more consistently delay the various stages of hydration reaction and reduce heat development, thus potentially becoming a better choice for cement modification materials.
[0100] It can be seen from this that the nanofluid admixture in the present invention can slow down the setting of the slurry, reduce the heat of hydration and optimize the pore structure. In addition, it has high dispersibility, low cost and is easy to apply on a large scale.
[0101] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. Application of a nanofluid admixture in clean slurry.
2. The use according to claim 1, characterized in that: The specific method of the application is: adding the nanofluid admixture into cement paste to obtain modified cement paste.
3. The use according to claim 2, characterized in that: The nanofluid admixture contains a surfactant, and the surfactant is at least one of polyvinyl alcohol and sodium carboxymethyl cellulose.
4. The use according to claim 3, characterized in that: The mass fraction of graphene in the nanofluid admixture is 0.02% to 0.12%; the mass fraction of the nanofluid admixture in the modified pure slurry is 0.05% to 0.08%.
Citation Information
Patent Citations
Graphene modified cement-based composite material and preparation method thereof
CN109553366A
Low-temperature-rise, high-impermeability and low-carbon concrete nano-fluid admixture as well as preparation method and application thereof
CN119349919A