A high-crack-resistant and radiation-resistant large-volume concrete and preparation method thereof

By modifying boron-containing mine tailings and using aggregate icing and cooling measures, high-crack-resistant and radiation-resistant large-volume concrete was prepared, which solved the shortcomings of nuclear power concrete in terms of large volume and crack resistance, improved radiation protection performance, and achieved efficient resource utilization.

CN117447149BActive Publication Date: 2024-11-15CHINA CONSTR WEST CONSTR SOUTHWEST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311235929.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-25
Publication Date
2024-11-15
Estimated Expiration
2043-09-25

AI Technical Summary

Technical Problem

Existing nuclear power plant concrete is insufficient in terms of large volume and high crack resistance, and the resources of boron-containing mine tailings are not fully utilized, resulting in poor radiation protection performance.

Method used

By modifying boron-containing mine tailings and using aggregate icing cooling measures, combined with modified clay, the radiation resistance and crack resistance of concrete are improved, and high-crack-resistant and radiation-resistant large-volume concrete is prepared.

Benefits of technology

It effectively improves the radiation resistance and crack resistance of concrete, reduces the heat of hydration, reduces the possibility of temperature cracks, and achieves efficient utilization of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-crack-resistant and radiation-resistant large-volume concrete, which is composed of the following components by weight: 250-300 parts of cement, 10-30 parts of modified boron-containing mine tailings, 60-90 parts of Class II fly ash, 600-900 parts of ordinary sand, 250-1250 parts of cooling aggregate, 250-1250 parts of normal-temperature aggregate, and 165 parts of water; the modified boron-containing mine tailings are industrial waste slag discharged after borax production from boron-magnesium ore, which is obtained by grinding after high-temperature calcination modification; the ignition loss is 20%-30%; the MgO content in the chemical composition is The invention discloses a method for treating and modifying boron-containing mine tailings to increase the utilization efficiency of the boron-containing mine tailings in radiation-resistant concrete, and especially improve the shrinkage cracking resistance of the boron-containing mine tailings in the concrete. The method comprises the following steps: applying ice to the coarse aggregate to reduce the temperature, thereby effectively ensuring the temperature of the concrete before it is poured out of the concrete machine; and combining the physical and chemical properties of the modified boron-containing mine tailings, the aggregate ice-covered cooling and the modified clay to effectively improve the radiation resistance and cracking resistance of the large-volume concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete materials, and in particular relates to a high-crack-resistant and radiation-resistant large-volume concrete and a preparation method thereof. Background Art

[0002] Due to traditional historical reasons and resource limitations, a large part of my country's electricity comes from fossil energy such as coal-fired power generation. However, the utilization rate of coal-fired power generation is low, which has caused serious air pollution and is the main source of greenhouse gas emissions. Nuclear power, as an efficient and clean new energy source, has unique advantages and is an inevitable choice for optimizing the energy use structure. We must correctly deal with the problems brought by nuclear energy. A large number of rays produced by nuclear energy nuclear reactions, such as α, β, γ, X-rays and neutron rays, can induce a variety of diseases and gene mutations, posing a great threat to the environment and human health. In order to prevent the harm of radiation to the human body and the environment, protective bodies must be set up when building buildings with radiation sources. Cement concrete is currently the most widely used radiation protection material, such as the inner and outer shells of nuclear reactors and the solidification of nuclear waste. At present, the main radiation protection materials used for radiation protection are steel plates, lead plates, water and concrete. Considering the source, cost and implementation difficulty of these materials, among these radiation protection materials, the comprehensive technical and economic effect of concrete is undoubtedly the best.

[0003] On the other hand, the current methods of enhancing the radiation protection of concrete mainly include: 1. increasing the heavy metal content in a single cubic meter of concrete; 2. increasing the light element content of the solution in the concrete, etc. With the development of nuclear energy, there are more and higher requirements for nuclear power concrete, such as larger volume, high crack resistance and constant temperature. Therefore, by preparing a low-temperature, high-crack resistance and large-volume nuclear power concrete, it will be of great significance to improve the diversity and adaptability of nuclear power concrete.

[0004] Boron-containing mine tailings are industrial waste residues discharged after borax is produced from boron magnesium (iron) ore. The country produces more than one million tons of boron-containing mine tailings each year, which causes serious pollution. Therefore, it is very necessary and urgent to recycle and reuse boron-containing mine tailings in a large-scale and new form to fundamentally solve the pollution problem of boron-containing mine tailings. Chinese invention patent CN 104817304 discloses a method for preparing radiation-resistant concrete from boron-containing mine tailings, which improves the radiation resistance of concrete by directly adding boron-containing mine tailings to concrete. However, the invention does not fully and efficiently utilize all the chemical substances contained in the boron-containing mine tailings. Summary of the invention

[0005] The purpose of the present invention is to provide a high-cracking and radiation-resistant large-volume concrete and a preparation method thereof, to treat and modify boron-containing mine tailings, to increase their utilization efficiency in radiation-resistant concrete, and in particular to improve their resistance to shrinkage cracking in concrete; by means of ice-coating and cooling measures for coarse aggregates, the discharge and pouring temperatures of the concrete can be effectively guaranteed; and at the same time, the physical and chemical properties of modified boron-containing mine tailings, aggregate ice-coating and cooling, and modified clay are combined to effectively improve the radiation resistance and cracking resistance of large-volume concrete.

[0006] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0007] A high crack-resistant and radiation-resistant mass concrete, the composition of which is as follows by weight:

[0008] 250-300 parts of cement, 10-30 parts of modified boron-containing mine tailings, 60-90 parts of grade II fly ash, 600-900 parts of ordinary sand, 250-1250 parts of cooling aggregate, 250-1250 parts of room temperature aggregate, and 165 parts of water.

[0009] According to the above scheme, the cement used is P·O 42.5 cement, 300m 2 / kg≤Specific surface area≤370m 2 / kg.

[0010] According to the above scheme, the modified boron-containing mine tailings are industrial waste slag discharged after producing borax from boron-magnesium ore, which is modified by high-temperature calcination and then ground; the loss on ignition is 20%-30%; the MgO content in the chemical composition is 40-50wt%, and the B2O3 content is 25~40wt%; the average particle diameter is 20-50μm.

[0011] According to the above scheme, the high-temperature calcination temperature of the modified boron-containing mine tailings is 600-1100°C and the calcination time is 30min-60min. At the same time, the specific calcination temperature and time are determined by the content of internal magnesium oxide and light-burned magnesium and the activity of the boron-containing tailings.

[0012] According to the above scheme, the cooling aggregate is obtained by cooling the piled normal temperature aggregate by ice coating; the aggregate stacking thickness is 2-2.5m, the aggregate ice coating thickness range is 0.1m-0.3m, the ice coating duration is 2d-4d, and the aggregate temperature range after ice coating is 18-22℃.

[0013] According to the above scheme, the ordinary sand is medium-coarse sand, and its fineness modulus is between 2.3-3.0.

[0014] According to the above scheme, the fineness range of the Class II fly ash is 30-40%, the loss on ignition range is 3%-8%, the chemical composition includes CaO content of 4-10%, K2O content of 1-4%, SiO2 content of 45-55%, Fe2O3 content of 3%-8%, and Al2O3 content of 25%-35%.

[0015] The method for preparing the above-mentioned high crack-resistant and radiation-resistant large-volume concrete comprises the following steps:

[0016] Pour cooling aggregate, room temperature aggregate, cement, Class II fly ash, modified boron-containing mine tailings and ordinary sand into a mixer and mix evenly, then add water and mix evenly to obtain high crack-resistant and radiation-resistant large-volume concrete.

[0017] According to the characteristics of relevant elements in boron-containing mine tailings, the present invention modifies the boron-containing mine tailings and further utilizes them in the preparation of large-volume nuclear power concrete, effectively improving the crack resistance and radiation resistance of concrete. Specifically: 1. When the boron-containing mine tailings are heated at high temperatures, the magnesite contained in them will decompose to obtain magnesium oxide or light-burned magnesium (i.e., MgCO3=MgO+CO2, magnesite will begin to decompose into magnesium oxide and carbon dioxide after being heated to above 640°C, and after heating to 750-1000°C, the carbon dioxide does not completely overflow, and the product is a powdery substance, which is light-burned magnesium), which can effectively improve the crack resistance of concrete; 2. Boron-containing mine tailings contain a high content of boron-containing compounds (B2O3), which can be added to concrete to effectively improve the radiation resistance of concrete.

[0018] The invention processes and modifies the boron-containing mine tailings to increase the utilization efficiency of the tailings in radiation-resistant concrete, and especially improves the shrinkage cracking resistance of the tailings in the concrete.

[0019] The present invention adopts the coarse aggregate icing cooling measure, which can effectively ensure the temperature of concrete out of the machine and pouring. In addition, through theoretical calculation, the temperature of the coarse aggregate used in the concrete is controlled by means of adjusting the icing time and quantity, so that the cooling aggregate can maintain a low temperature during the hydration reaction of the concrete (15-30h), thereby completing the physical thermal process, reducing the hydration heat of large-volume concrete, and further reducing the possibility of concrete cracking.

[0020] The present invention organically combines the physical and chemical properties of modified boron-containing mine tailings, aggregate ice-coating cooling and modified clay, not only effectively improving the radiation resistance and cracking resistance of large-volume concrete, but also provides a high-cracking and radiation-resistant large-volume concrete with cement, boron-containing mine tailings and modified clay as main components and a preparation method thereof, thus making resource utilization of boron-containing mine tailings and clay, and having great application prospects.

[0021] The inventors found in the long-term work process of nuclear power projects that when pouring important concrete parts, the performance and temperature of concrete are required to be high. For example, in terms of concrete temperature, the pouring temperature needs to be kept at room temperature all year round, which creates great difficulties and impacts on summer concrete production and construction. The present invention makes full use of the characteristics that the amount of coarse aggregate (stone) used in a single cubic meter of concrete is much greater than the amount of water, and the specific heat capacity is larger than that of other materials except water, and the heat conductivity rate is relatively low. The coarse aggregate is pre-cooled to keep the temperature rise rate of the concrete at a low level after mixing and leaving the machine, thereby ensuring that the pouring temperature of the concrete is qualified (the temperature rise of one cubic meter of concrete aggregate is equivalent to the temperature rise of 3°C of water) (calculate the total heat absorption of the stone in one cubic meter of concrete is greater than the heat absorption of water).

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] In terms of radiation resistance, the present invention uses modified boron-containing mine tailings, which are obtained by grinding the industrial waste slag discharged after producing borax from boron-magnesium ore after high-temperature calcination. It has a large amount of boron-containing compounds (B2O3), which can be added to concrete to improve the ability to absorb nuclear radiation and effectively improve the radiation resistance. In addition, the boron-magnesiumite that is not easy to alkali hydrolyze in the boron-containing mine tailings after direct roasting is decomposed into suian stone that is easy to alkali hydrolyze after roasting and dehydration, and the activity of the boron-containing compound (B2O3) is further improved, thereby greatly improving the radiation resistance of the prepared concrete.

[0024] In terms of crack resistance, the modified boron-containing mine tailings used in the present invention contain a high content of magnesium oxide and light-burned magnesium (magnesite begins to decompose into magnesium oxide and carbon dioxide after being heated to above 640°C. After heating to 750-1100°C, the carbon dioxide does not completely overflow, and the product is a powdery substance, which is light-burned magnesium). Magnesium oxide and light-burned magnesium are important components of the expansion agent, which play a role in inhibiting the occurrence of cracks in the concrete during development; in addition, due to the high internal hydration heat release of large-volume concrete, the possibility of concrete cracks is greatly increased, and the highest hydration heat release time is between 20-30h after casting. At the same time, in the summer ambient temperature, it takes about 40h for the cooling aggregate to rise from 20°C to 30°C. Therefore, the cooling aggregate used in the present invention has the function of absorbing heat during the hydration heat release process of concrete, which can reduce the internal hydration heat of concrete and reduce the possibility of temperature cracks.

[0025] In terms of high temperature resistance, the forsterite component contained in the ground modified boron-containing mine tailings used in the present invention can effectively improve the high temperature resistance of concrete. After being applied to nuclear power concrete, it can play a better protective role and improve the safety performance of nuclear power projects. DETAILED DESCRIPTION

[0026] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.

[0027] The specific implementation method provides a high crack resistance and radiation resistance mass concrete, the composition of which is as follows by weight:

[0028] 250-300 parts of cement, 10-30 parts of modified boron-containing mine tailings, 60-90 parts of grade II fly ash, 600-900 parts of ordinary sand, 250-1250 parts of cooling aggregate, 250-1250 parts of room temperature aggregate, and 165 parts of water.

[0029] Specifically, cement used is P·O 42.5 cement, 300m 2 / kg≤Specific surface area≤370m 2 / kg.

[0030] Specifically, the modified boron-containing mine tailings are industrial waste slag discharged after producing borax from boron-magnesium ore, which is modified by high-temperature calcination and then ground; the loss on ignition is 20%-30%; the MgO content in the chemical composition is 40-50wt%, and the B2O3 content is 25~40wt%; the average particle diameter is 20-50μm.

[0031] Specifically, the high-temperature calcination temperature of the modified boron-containing mine tailings is 600-1000°C and the calcination time is 30min-120min. At the same time, the specific calcination temperature and time are determined by the content of internal magnesium oxide and light-burned magnesium.

[0032] The high-temperature calcination time of the boron-containing mine tailings used in this embodiment is 90 minutes.

[0033] Specifically, the cooling aggregate is obtained by coating the piled normal temperature aggregate with ice to cool it down; the aggregate stacking thickness is 2-2.5m, the aggregate ice coating thickness ranges from 0.1m to 0.3m, the ice coating duration is 2d to 4d, and the aggregate temperature ranges from 18 to 22°C after ice coating.

[0034] Specifically, ordinary sand is medium-coarse sand, and its fineness modulus is between 2.3-3.0.

[0035] Specifically, the fineness range of Class II fly ash is 30-40%, the loss on ignition range is 3%-8%, the chemical composition includes CaO content of 4-10%, K2O content of 1-4%, SiO2 content of 45-55%, Fe2O3 content of 3%-8%, and Al2O3 content of 25%-35%.

[0036] The mix proportion of the highly crack-resistant and radiation-resistant large-volume concrete in the specific embodiment is shown in Table 1, and the water-cement ratio is fixed at 0.46, which is similar to the water-cement ratio of the C30 large-volume concrete mix proportion in the actual nuclear power project.

[0037] Table 1

[0038]

[0039] The performance characteristics of concrete obtained in each specific embodiment are shown in Table 2. The adiabatic temperature rise of concrete was tested according to the provisions of GB / T 50080-2016 "Standard for Performance Test Methods of Ordinary Concrete Mixtures". The performance analysis of concrete shielding γ-rays was carried out by measuring the absorbed dose rate of the concrete slab at a distance of 40 cm from the radiation source and 5 cm from the back of the concrete slab to the detector. The linear absorption rate was then calculated theoretically.

[0040] Table 2

[0041] serial number Slump / mm Expansion / mm 28d compressive strength / MPa Adiabatic temperature rise value / ℃ <![CDATA[Flat cracking area / m 2 > Gamma rays (2.0 MeV) Neutron radiation (10 MeV) 1 180 510 45.7 59.8 409.8 0.24 0.32 2 180 520 46.2 60.1 320.6 0.26 0.34 3 185 510 43.6 57.6 251.2 0.30 0.42 4 190 530 42.4 55.2 218.6. 0.34 0.46 5 185 520 38.5 54.1 186.7 0.41 0.52 6 195 500 37.0 58.4 431.5 0.25 0.31 7 185 530 41.9 56.3 220.3 0.30 0.42 8 190 520 45.5 55.9 215.3 0.32 0.44 9 180 540 44.0 56.2 210.1 0.30 0.41 10 185 530 42.3 55.6 214.4 0.29 0.39 11 175 510 40.4 56.3 209.2 0.27 0.36 12 180 520 39.2 55.7 198.6 0.35 0.43 13 175 510 41.0 54.3 210.5 0.34 0.45 14 180 500 43.1 50.6 216.7 0.35 0.47 15 180 510 40.8 48.9 204.8 0.32 0.45 16 185 530 38.9 47.2 192.2 0.33 0.42

[0042] It can be seen from the test data that the concrete specimens of the embodiments of the present invention show good crack resistance, reduced hydration heat and radiation resistance, and maintain good working performance and mechanical properties. Among them, it can be seen from the comparative examples and Examples 2-5 that the addition of modified boron-containing waste powder can effectively improve the gamma-ray and neutron ray resistance of concrete, wherein as the dosage of modified boron-containing waste powder gradually increases, the linear attenuation coefficient of concrete continues to decrease, which is due to the gradual increase in dosage, the B2O3 content in concrete also gradually increases, effectively enhancing the radiation resistance of concrete; Observation of Examples 4 and 7-11 shows that with the increase in the calcination temperature of the boron-containing tailings, the radiation resistance of concrete shows a trend of first strengthening and then weakening, and when the temperature is about 700°C, its radiation resistance is the best; In addition, further analysis of the change law of the crack resistance of concrete shows that with the gradual increase in the dosage of modified boron-containing waste powder, the crack resistance of concrete is significantly improved, which is due to the continuous increase in the MgO content inside the concrete, and the delayed expansion of MgO hydration effectively improves the crack resistance of concrete.

[0043] In addition, further observation of Comparative Example 1 and Examples 12-16 shows that as the amount of cooling aggregate continues to increase, the adiabatic temperature rise value of the concrete continues to decrease. The reason is that after the aggregate is cooled by ice, it will be able to absorb the heat released during cement hydration, thereby reducing the hydration heat inside the concrete, thereby reducing the possibility of temperature cracks in the concrete.

[0044] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

Claims

1. A high crack-resistant and radiation-resistant mass concrete, characterized in that The composition is calculated by weight as follows: 250-300 parts of cement, 10-30 parts of modified boron-containing mine tailings, 60-90 parts of Class II fly ash, 600-900 parts of ordinary sand, 250-1250 parts of cooling aggregate, 250-1250 parts of room temperature aggregate, and 165 parts of water; The modified boron-containing mine tailings are obtained by grinding industrial waste slag discharged after producing borax from boron-magnesium ore after high-temperature calcination modification; the ignition loss is 20%-30%; the MgO content in the chemical composition is 40-50wt%, the B2O3 content is 25-40wt%; and the average particle diameter is 20-50μm.

2. The high crack-resistant and radiation-resistant mass concrete according to claim 1, characterized in that The cement used is P·O 42.5 cement, 300m 2 / kg≤Specific surface area≤370m 2 / kg.

3. The high crack-resistant and radiation-resistant mass concrete according to claim 1, characterized in that The high-temperature calcination temperature of the modified boron-containing mine tailings is 600-1100° C., and the calcination time is 30 min-120 min.

4. The high crack-resistant and radiation-resistant mass concrete according to claim 1, characterized in that The cooling aggregate is obtained by cooling the piled normal temperature aggregate by ice coating; the aggregate stacking thickness is 2-2.5m, the aggregate ice coating thickness ranges from 0.1m to 0.3m, the ice coating duration is 2d to 4d, and the aggregate temperature ranges from 18 to 22°C after ice coating.

5. The highly crack-resistant and radiation-resistant mass concrete according to claim 1, characterized in that The ordinary sand is medium-coarse sand, and its fineness modulus is between 2.3 and 3.

0.

6. The high crack-resistant and radiation-resistant mass concrete according to claim 1, characterized in that The Class II fly ash has a fineness range of 30-40%, a loss on ignition range of 3%-8%, a chemical composition of CaO content of 4-10%, a K2O content of 1-4%, a SiO2 content of 45-55%, a Fe2O3 content of 3%-8%, and an Al2O3 content of 25%-35%.

7. The method for preparing the highly crack-resistant and radiation-resistant mass concrete according to any one of claims 1 to 6, characterized in that The following steps are involved: Pour cooling aggregate, room temperature aggregate, cement, Class II fly ash, modified boron-containing mine tailings and ordinary sand into a mixer and mix evenly, then add water and mix evenly to obtain high crack-resistant and radiation-resistant large-volume concrete.