Composite additive for gypsum material and preparation method thereof
By using composite additives of polyethylene oxide and triethanolamine in gypsum materials, the structural stability of the bubble body is enhanced, and the problem of compressive strength attenuation of gypsum foam material is solved under the freeze-thaw cycle, achieving efficient anti-freeze Durability and versatility performance improvements.
Patent Information
- Application Number
- CN202411002957.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
Gypsum foaming materials have severe tensile and compressive strength attenuation under the freeze-thaw cycle in cold areas, making it difficult to meet the durability requirements of building walls.
The composite additives of polyethylene oxide, triethanolamine, nanocellulose ether, potassium aluminum sulfate dodecano, ethylene diphosphate and anhydrous calcium chloride are used to adjust the structure of gypsum materials and enhance the structural stability of bubbles. and compressive strength, and through the preparation method, ensure uniform dispersion of components to form round and uniform bubbles.
The gypsum material has been damaged and maintained with compressive strength after 15 freeze-thaw cycles, complies with the national standards for freezing resistance, and improves the waterproof, moisture-proof, fire-proof, sound-proof and thermal conductivity of the material.
Smart Images

Figure CN118930123A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and in particular relates to a composite additive for gypsum materials and a preparation method thereof. Background Art
[0002] The durability of building materials has become a focus of attention in the engineering community, especially in cold areas. Damage and deterioration caused by freeze-thaw cycles will affect the durability of the structure. Therefore, the "Autoclaved Aerated Concrete Blocks" (GB / T11968-2020) requires that the strength loss is less than 20% after 15 freeze-thaw cycles.
[0003] The development of lightweight, high-strength, porous inorganic thermal insulation materials using gypsum (natural gypsum, solid waste gypsum) as raw materials is a very promising direction. At present, the method and process of gypsum foaming materials are simple. Generally, foaming is achieved by adding a foaming agent to the gypsum and then reacting and expanding it. Since the introduced bubbles increase the interface of the gypsum slurry, the system is prone to instability, which directly affects the performance of the gypsum foaming material.
[0004] Freeze-thaw has a great influence on the tensile and compressive strength of gypsum foam materials. With the increase of freeze-thaw cycles, the attenuation degree of tensile and compressive strength increases.
[0005] Based on this, the present invention aims to study a gypsum material composite additive, apply it to gypsum material, make its structure have better frost resistance, increase the frost resistance durability of gypsum material, so as to meet the application requirements of building walls, internal and external insulation materials, especially the requirements of exterior walls. Summary of the invention
[0006] In view of the above-mentioned technical problems and the shortcomings in the art, the present invention provides a composite additive for gypsum materials. The composite additive of the present invention is used to adjust the structure of the gypsum material and enhance the stability of the foam structure, thereby achieving good anti-freeze durability. After 15 freeze-thaw cycle tests, the specimen is not damaged and still has compressive strength after freeze-thaw.
[0007] The object of the present invention is to provide a composite additive for gypsum materials, comprising the following components in percentage by mass:
[0008]
[0009]
[0010] The polyethylene oxide and triethanolamine of the present invention are mainly used as film-forming substances of the foam, which can fully improve the compressive strength of the inorganic foamed gypsum material, and triethanolamine has the function of stabilizing the foam structure, and obtains the mutually unconnected foam tissue through silicone amide, and controls the number and size of the foam with components such as nanocellulose ether, and the obtained foam is round and the bubbles are uniform; potassium aluminum sulfate dodecahydrate mainly serves to enhance the waterproof function, and at the same time has the function of enhancing the compressive strength; hydroxyethylidene diphosphonic acid has a stable structure and is not easy to hydrolyze; anhydrous calcium chloride enables the inorganic foamed gypsum composite material to maintain acid-base balance and increase the compactness of the foam wall. By adopting the composite additive of the present invention to adjust the structure of the gypsum material and enhance the stability of the foam structure, good antifreeze durability is achieved, and the test piece is not damaged after 15 freeze-thaw cycle tests and still has compressive strength after freeze-thaw.
[0011] Furthermore, the molecular weight of polyethylene oxide is 50,000-150,000, and the molecular weight of nanocellulose ether is 5,000-20,000.
[0012] The present invention also aims to provide a method for preparing a composite additive for gypsum materials, comprising the following steps:
[0013] (1) Weigh each component according to the ratio, add water into a reaction container, add sodium molybdate, disperse and mix evenly, add polyethylene oxide, and disperse and mix evenly after the polyethylene oxide is completely wetted;
[0014] (2) adding nanocellulose ether, triethanolamine, silicone amide and pentaerythritol, and dispersing and mixing them evenly;
[0015] (3) adding potassium aluminum sulfate dodecahydrate, hydroxyethylidene diphosphoric acid, sodium pyrophosphate, anhydrous calcium chloride and dimethyl silicone oil, dispersing and mixing them evenly to obtain a composite additive for gypsum materials.
[0016] Furthermore, in step (1), the first dispersing stirring speed is 1300-1600 r / min, and the dispersing stirring time is 50-65 min; in step (2), the second dispersing stirring speed is 1300-1600 r / min, and the dispersing stirring time is 15-45 min; in step (3), the third dispersing stirring speed is 1300-1600 r / min, and the dispersing stirring time is 15-45 min.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The composite additive of the present invention enables the prepared gypsum material to have a water-blocking function, preventing a large amount of water molecules from entering the interior of the gypsum material foam. At the same time, the wall thickness density of the foam wall is increased to make the foam stronger and more airtight, preventing the penetration of water molecules, making the foam structure more stable, so that the foam will not be squeezed and deformed due to the expansion force and contraction force generated by the alternation of cold and hot (-15°C to 105°C). As a result, the frost resistance and durability of the gypsum material prepared by using the composite additive of the present invention are greatly improved, and the strength loss rate of the gypsum product after 15 freeze-thaw cycles is less than 20%, which meets the requirements of the national standard "Autoclaved Aerated Concrete Block" (GB / T 11968-2020) for frost resistance, and can be used as building walls, internal and external insulation materials, especially exterior walls;
[0019] (2) The polyethylene oxide and triethanolamine used in the present invention are mainly used as film-forming substances for the foamed body, which fully improve the compressive strength of the inorganic gypsum material prepared by using the composite additive. The polyanionic cellulose is used to adjust the number of foams according to the amount of its addition to enhance the compressive strength. The wall thickness of the mutually unconnected foams of the inorganic gypsum composite material prepared by the composite additive is adjusted by using materials such as hydrogen peroxide. The magnesium sulfate heptahydrate not only has a foaming catalytic effect in the inorganic gypsum composite material, but also improves the hardness of the inorganic gypsum composite material. The prepared gypsum material is a light and high-strength material with good mechanical strength, and the compressive strength can reach 9MPa.
[0020] (3) Compared with ordinary gypsum materials, the inorganic gypsum composite material prepared by using the composite additive of the present invention has light weight and convenient construction. It can be used for heat preservation and has good heat preservation and sound insulation effects. The thermal conductivity can be as low as 0.02W / m·K, and the sound insulation and noise reduction test reaches 45dB. It has a certain protective effect (shielding effect) on some low-frequency electromagnetic waves (such as power line radiation). Other protective materials (such as metal) can also be added to achieve high-frequency electromagnetic radiation shielding. Gypsum, as a porous material, has high water absorption and water permeability. The material prepared by this application enhances the waterproof and moisture-proof properties, and the water absorption rate is reduced to 5%;
[0021] (4) The inorganic gypsum composite material prepared by the composite additive of the present invention has a crystal structure and high stability, which enables it to withstand high temperatures up to 1700°C. Its fire protection is achieved by absorbing heat. When a fire occurs, the gypsum composite material can absorb heat energy, reduce the ambient temperature, and delay the spread of the fire. The fire protection level is A1; the fire extinguishing function is that the inorganic gypsum composite material is an A1 non-combustible material, the product is heat-insulating and flame-retardant, and is a poor conductor of heat. In the event of a fire, less heat is transferred to the back-fire surface, and its equilibrium temperature is low, which can avoid the back-fire surface temperature rising and reaching the ignition point or igniting other objects for a long time. Even if the fire-facing surface of the inorganic gypsum composite material is burned at high temperature for 3.5 hours, the temperature of the side facing away from the fire will not exceed 50°C, which effectively plays a role of fire insulation and flame retardancy. The gypsum product prepared by the composite additive of the present invention is resistant to high temperature, heat insulation and fire prevention, does not catch fire, does not smolder, and does not carbonize. It belongs to A1 grade fireproof material and can be widely used in various high-rise residential buildings and other civil buildings. The protective layer of the internal and external insulation system. In addition, the gypsum filler using this additive has the effects of corrosion resistance, high temperature resistance, easy construction, and fireproof and heat insulation compartments, which can improve the corrosion resistance of the material, so that the gypsum product can maintain good stability under continuous high temperature and extend the service life;
[0022] (5) Compared with organic high temperature resistant fillers, the inorganic gypsum composite material prepared by using the composite additive of the present invention is a non-toxic, green and environmentally friendly inorganic raw material because the gypsum is directly taken from nature and waste. The pollution to the environment during the production and use of the inorganic material is relatively small. The product uses water as the dispersion medium and has no adverse effects on environmental protection and health. In the event of a fire, the inorganic gypsum composite material only releases crystal water and converts into water vapor. It will not produce any toxic suffocating combustion gas, nor will it volatilize any decomposed or combustion-supporting substances and smoke, which can also reduce casualties when a fire occurs. The gypsum material prepared by using the composite additive for gypsum material of the present invention has the advantages of being green, environmentally friendly, and natural and non-toxic;
[0023] (6) The gypsum composite material prepared by using the composite additive of the present invention has recyclability. The present invention only uses inorganic raw materials to foam the gypsum, thereby obtaining high compressive strength and excellent frost resistance. In this process, no concrete or similar gel materials are added, and pure gypsum is used for foaming. Therefore, the present invention has good recyclability. The gypsum products produced by using the composite additive of the present invention can be completely recycled and reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The gypsum composite material prepared in Application Example 1 of the present invention;
[0025] Figure 2 This is the gypsum material prepared in Comparative Example 1. DETAILED DESCRIPTION
[0026] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1 Preparation of composite additives for gypsum materials
[0028] (1) Weigh by mass percentage: 38.7% water, 0.25% sodium molybdate, 2% polyethylene oxide (molecular weight 100,000), 5% nanocellulose ether (molecular weight 10,000), 15% triethanolamine, 5% pentaerythritol, 0.05% dimethyl silicone oil, 2% anhydrous calcium chloride, 2% silicone amide, 10% sodium pyrophosphate, 10% hydroxyethylidene diphosphonic acid, and 10% potassium aluminum sulfate dodecahydrate.
[0029] First, add a certain amount of water to the reactor, set the reactor temperature to 70°C, set the disperser speed to 500r / min, add sodium molybdate, set the disperser speed to 1500r / min, wait for the reaction temperature to reach the set value of 70°C, and disperse for 10 minutes. Adjust the reactor temperature to 25°C, reduce the disperser speed to 500r / min, and then add polyethylene oxide. After the polyethylene oxide is fully wetted, increase the disperser speed (called the first disperser stirring speed) to 1500r / min, and the dispersion time is 60 minutes.
[0030] (2) Then, the speed of the disperser was set to 500 r / min, and nanocellulose ether, triethanolamine, silicone amide, and pentaerythritol were added in sequence. The speed of the disperser (referred to as the second disperser speed) was set to 1500 r / min, and the dispersion time was 30 minutes.
[0031] (3) Finally, the disperser speed is set to 650 r / min, and potassium aluminum sulfate dodecahydrate, hydroxyethylidene diphosphoric acid, sodium pyrophosphate, anhydrous calcium chloride, and dimethyl silicone oil are added in sequence. The disperser speed (called the third disperser stirring speed) is set to 1500 r / min, and the mixture is dispersed for 20 minutes. The reactor is closed and cooled to room temperature to obtain a composite additive for gypsum materials.
[0032] Polyethylene oxide and triethanolamine are mainly used as film-forming substances for foams, which can fully improve the compressive strength of inorganic foamed gypsum materials and prevent the product from falling off after solidification. Triethanolamine has the functions of adjusting construction viscosity, pH value, reducing water, and stabilizing foam structure. Silicone amide and nanocellulose ether can control the number and size of foams; hydroxyethylidene diphosphonic acid can effectively inhibit the catalytic decomposition of hydrogen peroxide caused by metal ions. Sodium pyrophosphate mainly acts as a hydrogen peroxide stabilizer and can improve the strength of inorganic gypsum composite materials; pentaerythritol mainly acts as a surfactant, adhesive, and flame retardant; sodium molybdate is used as a foaming catalyst and corrosion inhibitor for metal materials to play an anti-corrosion role; anhydrous calcium chloride enables the inorganic foamed gypsum composite material to maintain acid-base balance and increase the density of the foam wall; dimethyl silicone oil is mainly used for penetration and defoaming.
[0033] Example 2
[0034] Weigh by mass percentage: 20.47% water, 0.5% sodium molybdate, 10% polyethylene oxide (molecular weight of 100,000), 10% nanocellulose ether (molecular weight of 10,000), 10% triethanolamine, 5% pentaerythritol, 0.03% dimethyl silicone oil, 2% anhydrous calcium chloride, 2% silicone amide, 15% sodium pyrophosphate, 15% hydroxyethylidene diphosphoric acid, and 10% potassium aluminum sulfate dodecahydrate. The preparation process is the same as that of Example 1.
[0035] Example 3
[0036] Weigh by mass percentage: 17.7% water, 0.2% sodium molybdate, 15% polyethylene oxide (molecular weight of 100,000), 5% nanocellulose ether (molecular weight of 10,000), 20% triethanolamine, 5% pentaerythritol, 0.1% dimethyl silicone oil, 2% anhydrous calcium chloride, 5% silicone amide, 10% sodium pyrophosphate, 10% hydroxyethylidene diphosphoric acid, and 10% potassium aluminum sulfate dodecahydrate. The preparation process is the same as that of Example 1.
[0037] Example 4
[0038] Weigh by mass percentage: 16.87% water, 0.1% sodium molybdate, 20% polyethylene oxide (molecular weight 100,000), 5% nanocellulose ether (molecular weight 10,000), 10% triethanolamine, 5% pentaerythritol, 0.03% dimethyl silicone oil, 2% anhydrous calcium chloride, 6% silicone amide, 10% sodium pyrophosphate, 10% hydroxyethylidene diphosphoric acid, and 15% potassium aluminum sulfate dodecahydrate. The preparation process is the same as that of Example 1.
[0039] The above embodiments are applied to gypsum materials to prepare gypsum composite materials.
[0040] Application Example 1 Preparation of gypsum composite materials
[0041] Weigh 50 parts of gypsum powder, 1.6 parts of magnesium sulfate heptahydrate, 32 parts of water, 1 part of the composite additive for gypsum materials prepared in Example 1, and 0.35 parts of hydrogen peroxide according to their mass fractions.
[0042] Add composite additives for gypsum materials and magnesium sulfate heptahydrate to the weighed water and mix them evenly with a mixer or disperser at a speed of 180 r / min; add gypsum powder after about 1 minute and disperse it with a mixer or disperser at a speed of 1000 r / min to make the gypsum powder and the solution fully mixed; add hydrogen peroxide after mixing for 2 minutes; pour into a mold or a filling product after dispersing for 1 minute, and cure to obtain an inorganic nano gypsum composite material.
[0043] The gypsum composite material prepared by this formula has a foaming ratio of 2 times and a measured density of 786.3kg / m 3 , thermal conductivity is 0.092W / m·K, sound insulation and noise reduction test reaches 31-45dB, and fire protection performance test reaches A1 level fire protection.
[0044] Application Example 2
[0045] Weigh 50 parts of gypsum powder, 1.6 parts of magnesium sulfate heptahydrate, 32 parts of water, 1 part of the composite additive for gypsum materials prepared in Example 2, and 0.35 parts of hydrogen peroxide. The preparation process is the same as that of Application Example 1.
[0046] The gypsum composite material prepared by this formula has a foaming ratio of 2.2 times and a measured density of 660.7kg / m 3 The thermal conductivity is 0.073W / m·K, the sound insulation and noise reduction test reaches 31-45dB, and the fire protection performance test reaches A1 level fire protection.
[0047] Application Example 3
[0048] Weigh 50 parts of gypsum powder, 1.6 parts of magnesium sulfate heptahydrate, 32 parts of water, 1 part of the composite additive for gypsum materials prepared in Example 3, and 0.35 parts of hydrogen peroxide. The preparation process is the same as that in Application Example 1.
[0049] The gypsum composite material prepared by this formula has a foaming ratio of 1.9 times and a measured density of 842.3kg / m 3 , thermal conductivity is 0.098W / m·K, sound insulation and noise reduction test reaches 31-45dB, and fire protection performance test reaches A1 level fire protection.
[0050] Application Example 4
[0051] Weigh 50 parts of gypsum powder, 1.6 parts of magnesium sulfate heptahydrate, 40 parts of water, 1 part of the composite additive for gypsum materials prepared in Example 4, and 0.35 parts of hydrogen peroxide. The preparation process is the same as that in Application Example 1.
[0052] The gypsum composite material prepared by this formula has a foaming ratio of 2.1 times and a measured density of 735.7 kg / m 3 , thermal conductivity is 0.078W / m·K, sound insulation and noise reduction test reaches 31-45dB, and fire protection performance test reaches A1 level fire protection.
[0053] Comparative Example 1
[0054] 100 parts by mass of hemihydrate gypsum, 50 parts by mass of anhydrous gypsum, 0.05 parts by mass of polycarboxylic acid aqueous agent, 0.1 parts by mass of polyethylene oxide, 0.05 parts by mass of protein retarder for gypsum, and 0.06 parts by mass of starch ether are added into a dry mixer and mixed evenly; then 8 parts by mass of sodium alkylbenzene sulfonate, 0.5 parts by mass of polyacrylamide, and 300 parts by mass of water are mixed evenly to obtain a foaming liquid, and the foaming liquid is placed in a foaming machine for foaming to form foam for 4 minutes; then 100 parts by mass of water is added to the mixed dry powder and stirred to obtain a mixed slurry; then the mixed slurry is evenly mixed with the foam and put into a mold for final shaping. The density of the gypsum material prepared as above is measured to be 403.1 kg / m 3 .
[0055] Performance test of application examples 1-4 and comparative example 1
[0056] 1. Internal structure comparison:
[0057] The gypsum composite material prepared in Application Example 1 is as follows Figure 1 As shown, Figure 2 This is the gypsum material prepared in comparative example 1. As can be seen from the figure, the gypsum composite material prepared in the application example of the present invention has uniform, dense and relatively regular shaped bubbles, and the stable bubble structure enables the gypsum composite material prepared in the present invention to have good antifreeze durability, while the conventional gypsum material prepared in comparative example 1, although it has a more substantial structure on the surface, basically does not have antifreeze durability.
[0058] 2. Freeze-thaw test:
[0059] Freeze-thaw test method (refer to the test experiment on frost resistance in "Test Method for Performance of Autoclaved Aerated Concrete" (GB / T 11969-2020)):
[0060] Freeze-thaw is to immerse the freeze-thaw specimen in a constant temperature water tank with a water temperature of (20±2)℃ for 48 hours. The water surface is at half the height of the freeze-thaw specimen for the first 24 hours, and the water surface is 30mm higher than the freeze-thaw specimen for the last 24 hours. Then take it out and put it in a sealed plastic bag and let it stand for 24 hours. Then put it in a low temperature box that has been cooled to (-15±2)℃ in advance. When the temperature drops to -15℃ again, record the time and keep it for no less than 8 hours before taking it out. The taken out freeze-thaw specimen is placed in a constant temperature and humidity box with a temperature of (20±2)℃ and a relative humidity of 95% and kept for no less than 6 hours. Freeze for 8 hours and thaw for 6 hours as a freeze-thaw cycle until the freeze-thaw specimen completes 15 freeze-thaw cycles. Place the freeze-thaw specimens after freeze-thaw in an electric forced air drying oven, keep them at (60±5)℃ for 24h, then keep them at (80±5)℃ for 24h, and then bake them at (105±5)℃ until constant quality. After sealing and cooling to room temperature, measure the compressive strength of the specimens.
[0061] The freeze-thaw test results are shown in the following table:
[0062]
[0063] The gypsum composite material prepared by the composite additive for gypsum materials of the present invention has significantly improved frost resistance compared with comparative example 1, and can pass 15 freeze-thaw tests. Comparative example 1 softens directly after the first freeze-thaw, and application examples 1-4 can not only pass 15 freeze-thaw tests, but also have a strength loss rate of less than 20%, which meets the requirements of the national standard "Autoclaved Aerated Concrete Block" (GB / T 11968-2020) for frost resistance. This shows that the gypsum material prepared by the composite additive for gypsum materials of the present invention has excellent frost resistance, and comparative example 1, which does not use the composite additive of the present invention, basically has no frost resistance.
[0064] Therefore, by adopting the composite additive for gypsum material of the present invention, the gypsum material has a water-blocking function, preventing a large number of water molecules from entering the interior of the foam of the gypsum material, and at the same time having uniform, dense and relatively regular foams, the wall thickness density of the foam wall is increased, making the foam stronger, and making the foam sealed, preventing the penetration of water molecules, making the structure of the foam more stable, so that it will not be squeezed and deformed due to the expansion force and contraction force generated by the alternation of hot and cold (-15°C to 105°C), thereby greatly improving the antifreeze durability of the gypsum material prepared by using the composite additive for gypsum material of the present invention, and achieving a strength loss rate of less than 20% after 15 freeze-thaw cycles, which meets the requirements of the national standard "Autoclaved Aerated Concrete Block" (GB / T 11968-2020) for antifreeze, and can be used as a material for building walls, especially exterior walls.
[0065] The above embodiments are only used to illustrate the present invention, rather than to limit the present invention. Those skilled in the relevant technical field may make various changes or modifications without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions should also belong to the scope of the present invention and should be defined by the claims.
Claims
1. A composite additive for gypsum material, characterized in that: The following components are included in mass percentage:
2. A composite additive for gypsum materials according to claim 1, characterized in that: The molecular weight of the polyethylene oxide is 50,000-150,000, and the molecular weight of the nanocellulose ether is 5,000-20,000.
3. A method for preparing a composite additive for gypsum materials according to claim 1 or 2, characterized in that: The following steps are included: (1) Weigh each component according to the ratio, add water into a reaction container, add sodium molybdate, disperse and mix evenly, add polyethylene oxide, and disperse and mix evenly after the polyethylene oxide is completely wetted; (2) adding nanocellulose ether, triethanolamine, silicone amide and pentaerythritol, and dispersing and mixing them evenly; (3) adding potassium aluminum sulfate dodecahydrate, hydroxyethylidene diphosphoric acid, sodium pyrophosphate, anhydrous calcium chloride and dimethyl silicone oil, dispersing and mixing them evenly to obtain a composite additive for gypsum materials.
4. The method for preparing the composite additive for paste foaming material according to claim 3, characterized in that: In step (1), the first dispersing stirring speed is 1300-1600 r / min, and the dispersing stirring time is 50-65 min; in step (2), the second dispersing stirring speed is 1300-1600 r / min, and the dispersing stirring time is 15-45 min; in step (3), the third dispersing stirring speed is 1300-1600 r / min, and the dispersing stirring time is 15-45 min.