Preparation method of high polymer damping composite material
By combining redispersed rubber powder and rubber powder with high-grade cement, silicone fume, and quartz sand in polymer damping composite materials, the problems of difficult and high cost in the existing technology are solved, and the material efficiency is achieved Preparation and excellent damping performance.
Patent Information
- Application Number
- CN202411006811.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
The processing of existing polymer damping composite materials is difficult and increases production costs.
By mixing the redispersed rubber powder and rubber powder in a specific proportion, adding high-grade cement, silicone fume and quartz sand, uniformly mixing and degassing using a mixer and vacuum degassing equipment, the processing difficulty of the material is reduced and the performance is achieved. Testing ensures that it meets the requirements.
It reduces production costs and significantly improves the damping performance, hardness and durability of the material. It is suitable for reducing vibration transmission in buildings and engineering structures and improving earthquake resistance.
Smart Images

Figure CN118930175A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of damping composite materials, in particular to a method for preparing a polymer damping composite material. Background Art
[0002] Polymer damping composite material is a composite material composed of polymer material and damping material. It has excellent damping performance and high strength. Polymer material is usually a material with high strength and wear resistance, while damping material is a material that can effectively absorb energy and reduce vibration. The combination of these two materials can give full play to their respective advantages and achieve better damping effect.
[0003] Currently available polymer damping composite materials usually have high hardness and strength, are difficult to process, and require special processing technology and equipment, which increases production costs. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention provides a method for preparing a polymer damping composite material, which solves the problems of great processing difficulty and increased production cost.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A method for preparing a polymer damping composite material, comprising the following specific steps:
[0006] Step 1: First prepare the following raw materials by mass percentage:
[0007] 5% to 15% redispersed rubber powder, 5% to 15% rubber powder, 30% to 40% high-grade cement, 5% to 15% silica fume and 15% to 20% quartz sand, then mix high-grade cement: silica fume: quartz sand in a ratio of 1:0.3:2 using a mixer, add appropriate amount of water and stir thoroughly to make cement slurry;
[0008] Step 2: Weigh and mix the redispersed rubber powder and rubber powder in a ratio of 1:0.5, add a small amount of water, and stir well to form a uniform rubber redispersed rubber powder mixture;
[0009] Step 3: slowly add the rubber redispersed rubber powder mixture prepared in step 2 to the cement slurry prepared in step 1, and stir evenly to make it fully mixed, and then add an appropriate amount of water reducing agent or retarder;
[0010] Step 4: Finally, pour the treated mixed material into the mold, compact and vibrate it with a press, use a vacuum degassing device to degas the slurry in the mold to remove bubbles and improve the density of the material, harden the treated composite material, wait for 24 to 36 hours for it to fully solidify, take out the solidified composite material, trim and polish it to make its surface smooth;
[0011] Step 5: After processing, the material is subjected to performance tests including damping performance, hardness, tensile strength, bending strength, and durability to ensure that it meets the requirements.
[0012] Preferably, the specific contents of the materials in step 1 are as follows:
[0013] The redispersed rubber powder is polyvinyl alcohol or polyacrylate, used as a binder, and the redispersed rubber powder is used to improve the strength and toughness of the material;
[0014] The rubber powder is styrene-butadiene rubber or polychloroprene rubber, which is the core of the damping material and provides the damping performance of the material. The rubber powder is used to reduce vibration energy;
[0015] The high-grade cement is P.O42.5, and the high-grade cement is used to provide strength and hardness of the material;
[0016] The silica fume is fly ash or slag powder, which is used as an admixture of high-grade cement to improve the crack resistance and durability of the material;
[0017] The quartz sand has a particle size range of 0.1 to 0.5 mm and is used to improve the strength and durability of the material.
[0018] Preferably, in step 1, the specific steps of mixing high-grade cement, silica fume and quartz sand are as follows:
[0019] Step 1: First, dry-mix cement and silica fume, then add water to mix, then add quartz sand and stir until uniform;
[0020] Step 2: Use a forced mixer to fully mix cement, silica fume, quartz sand and water to ensure the uniformity and fluidity of the concrete. The mixing time is 2 to 3 minutes.
[0021] Preferably, in step 2, the specific steps of mixing the redispersed rubber powder and the rubber powder are as follows:
[0022] Step 1: Make sure the operating environment is clean and has adequate ventilation, and prepare to disperse the rubber powder and rubber powder;
[0023] Step 2: Dry and grind the damp or agglomerated powder. After the powder is kept dry and dispersed, use accurate weighing equipment to weigh the required redispersed rubber powder and rubber powder for later use.
[0024] Step 3: Place the pre-treated redispersed rubber powder and rubber powder into a blender or mixing tank, start the mixing equipment, stir at a low speed first, and gradually increase the speed to ensure that the powders are evenly mixed. After mixing, take samples for quality inspection.
[0025] Preferably, in step 4, the vacuum degassing equipment comprises the following specific steps:
[0026] Step 1: Check whether the vacuum degassing equipment is intact and ensure that it is in normal working condition. Then pour the mixed slurry into the mold and place the mold on the workbench of the vacuum degassing equipment to ensure that the mold is sealed and connected to the equipment.
[0027] Step 2: Then start the vacuum degassing equipment, start vacuuming, observe the vacuum gauge, and stop vacuuming when the vacuum reaches the set value. The vacuum is between 0.05 and 0.1 bar.
[0028] Step 3: Keep the slurry in vacuum for a certain period of time to allow the bubbles in the slurry to fully escape. The degassing time is usually 10 to 30 minutes. Observe the surface of the slurry. When no more bubbles emerge, the degassing process is completed.
[0029] Step 4: Finally, slowly release the vacuum to avoid bubbles in the slurry due to pressure changes. After degassing is completed, remove the mold from the vacuum degassing equipment.
[0030] Preferably, in step 5, the performance test specifically includes the following contents:
[0031] Damping performance test: Use a dynamic mechanical analyzer and a vibration table to simulate the performance of polymer damping composite materials in a vibration environment. Analyze the dynamic mechanical properties of the material by applying dynamic loading and measuring the response. Measure the damping performance of polymer damping composite materials at different frequencies and temperatures, and determine the damping peak, damping bandwidth and damping temperature key parameters of the composite materials.
[0032] Hardness performance test: Use a hardness tester to measure the hardness of the material, which reflects the hardness and compressive resistance of the material. Place the hardness tester on the sample surface, apply a certain load, and measure the diameter or depth of the impression to calculate the hardness value of the material;
[0033] Bending strength and tensile strength performance test: Use a universal material testing machine to measure the tensile, compression, bending and shear mechanical properties of the material. Use a fixture to fix the sample on the testing machine, apply mechanical loading and measure the stress-strain curve of the material;
[0034] Durability performance test: A fatigue testing machine is used to evaluate the durability of materials under cyclic loads or vibration loading. Continuous loads or vibrations are applied and the deformation and damage of the material during repeated loading are observed.
[0035] The present invention provides a method for manufacturing a polymer damping composite material, which has the following beneficial effects:
[0036] 1. In the present invention, the redispersed rubber powder is mixed with the rubber powder, and the particles of the rubber powder are dispersed between the particles of the redispersed rubber powder. When the mixture is added to the cement slurry, the redispersed rubber powder is redispersed in water to form an emulsion, and the particles of the rubber powder are suspended in the emulsion, so that the processing difficulty is reduced, and there is no need to use professional equipment, thereby reducing the production cost.
[0037] 2. The present invention can effectively absorb impact energy and vibration energy by using redispersed rubber powder and rubber powder as elastic fillers, thereby significantly improving the damping performance of the material. When this material is used in buildings and engineering structures, it can effectively reduce vibration transmission and improve the seismic performance of the structure, thereby producing excellent damping performance.
[0038] 3. The present invention can improve the weather resistance and anti-aging ability of the material by adding silica fume and quartz sand, so that it can maintain stable performance under different environmental conditions, such as UV resistance and corrosion resistance. The high-grade cement as the basic material, combined with silica fume and quartz sand, can provide the high strength and durability required by the material. This composite material can not only withstand static and dynamic loads, but also maintain stable physical and chemical properties for a long time, so that the material has high strength and durability and excellent weather resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The present invention is a flow chart of a method for manufacturing a polymer damping composite material. DETAILED DESCRIPTION
[0040] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Embodiment 1:
[0042] Please refer to the attached Figure 1 The embodiment of the present invention provides a method for manufacturing a polymer damping composite material, comprising the following specific steps:
[0043] Step 1: First prepare the following raw materials by mass percentage:
[0044] 5% redispersed rubber powder, 10% rubber powder, 40% high-grade cement, 15% silica fume and 20% quartz sand, then take high-grade cement: silica fume: quartz sand in a ratio of 1:0.3:0.5 and mix them evenly with a mixer, add appropriate amount of water and stir well to make cement slurry;
[0045] Step 2: Weigh and mix the redispersed rubber powder and rubber powder in a ratio of 1:0.5, add a small amount of water, and stir well to form a uniform rubber redispersed rubber powder mixture;
[0046] Step 3: slowly add the rubber redispersed rubber powder mixture prepared in step 2 to the cement slurry prepared in step 1, and stir evenly to make it fully mixed, and then add an appropriate amount of water reducing agent or retarder;
[0047] Step 4: Finally, pour the treated mixed material into the mold, compact and vibrate it with a press, use a vacuum degassing device to degas the slurry in the mold to remove bubbles and improve the density of the material, harden the treated composite material, wait for 24 hours for it to fully solidify, take out the solidified composite material, trim and polish it to make its surface smooth;
[0048] Step 5: After processing, the material is subjected to performance tests including damping performance, hardness, tensile strength, bending strength, and durability to ensure that it meets the requirements.
[0049] The specific contents of the materials in step one are as follows:
[0050] The redispersible rubber powder is polyvinyl alcohol or polyacrylate, used as a binder, and is used to improve the strength and toughness of the material;
[0051] Rubber powder is styrene-butadiene rubber or polychloroprene rubber, which is the core of the damping material and provides the damping performance of the material. Rubber powder is used to reduce vibration energy;
[0052] High-grade cement is P.O42.5, and high-grade cement is used to provide strength and hardness to the material;
[0053] Silica fume is fly ash or slag powder. As an admixture of high-grade cement, silica fume is used to improve the crack resistance and durability of the material;
[0054] The particle size range of quartz sand is 0.15mm. Quartz sand is used to improve the strength and durability of materials.
[0055] In step 1, the specific steps of mixing high-grade cement, silica fume and quartz sand are as follows:
[0056] Step 1: First, dry-mix cement and silica fume, then add water to mix, then add quartz sand and stir until uniform;
[0057] Step 2: Use a forced mixer to fully mix cement, silica fume, quartz sand and water to ensure the uniformity and fluidity of the concrete. The mixing time is 2 minutes.
[0058] Preferably, in step 2, the specific steps of mixing the redispersed rubber powder and the rubber powder are as follows:
[0059] Step 1: Make sure the operating environment is clean and has adequate ventilation, and prepare to disperse the rubber powder and rubber powder;
[0060] Step 2: Dry and grind the damp or agglomerated powder. After the powder is kept dry and dispersed, use accurate weighing equipment to weigh the required redispersed rubber powder and rubber powder for later use.
[0061] Step 3: Place the pre-treated redispersed rubber powder and rubber powder into a blender or mixing tank, start the mixing equipment, stir at a low speed first, and gradually increase the speed to ensure that the powders are evenly mixed. After mixing, take samples for quality inspection.
[0062] In step 4, the specific steps of the vacuum degassing equipment are:
[0063] Step 1: Check whether the vacuum degassing equipment is intact and ensure that it is in normal working condition. Then pour the mixed slurry into the mold and place the mold on the workbench of the vacuum degassing equipment to ensure that the mold is sealed and connected to the equipment.
[0064] Step 2: Then start the vacuum degassing equipment, start vacuuming, observe the vacuum gauge, and stop vacuuming when the vacuum reaches the set value. The vacuum is at 0.05 bar;
[0065] Step 3: Keep the slurry in vacuum for a certain period of time to allow the bubbles in the slurry to fully escape. The degassing time is usually 15 minutes. Observe the surface of the slurry. When no more bubbles emerge, it means that the degassing process is completed.
[0066] Step 4: Finally, slowly release the vacuum to avoid bubbles in the slurry due to pressure changes. After degassing is completed, remove the mold from the vacuum degassing equipment.
[0067] In step 5, the performance test specifically includes the following:
[0068] Damping performance test: Use a dynamic mechanical analyzer and a vibration table to simulate the performance of polymer damping composite materials in a vibration environment. Analyze the dynamic mechanical properties of the material by applying dynamic loading and measuring the response. Measure the damping performance of polymer damping composite materials at different frequencies and temperatures, and determine the damping peak, damping bandwidth and damping temperature key parameters of the composite materials.
[0069] Hardness performance test: Use a hardness tester to measure the hardness of the material, which reflects the hardness and compressive resistance of the material. Place the hardness tester on the sample surface, apply a certain load, and measure the diameter or depth of the impression to calculate the hardness value of the material;
[0070] Bending strength and tensile strength performance test: Use a universal material testing machine to measure the tensile, compression, bending and shear mechanical properties of the material. Use a fixture to fix the sample on the testing machine, apply mechanical loading and measure the stress-strain curve of the material;
[0071] Durability performance test: A fatigue testing machine is used to evaluate the durability of materials under cyclic loads or vibration loading. Continuous loads or vibrations are applied and the deformation and damage of the material during repeated loading are observed.
[0072] Embodiment 2:
[0073] Please refer to the attached Figure 1 The embodiment of the present invention provides a method for manufacturing a polymer damping composite material, comprising the following specific steps:
[0074] Step 1: First prepare the following raw materials by mass percentage:
[0075] 15% redispersed rubber powder, 15% rubber powder, 35% high-grade cement, 15% silica fume and 20% quartz sand, then mix high-grade cement: silica fume: quartz sand in a ratio of 1:0.3:1 using a mixer, add appropriate amount of water and stir thoroughly to make cement slurry;
[0076] Step 2: Weigh and mix the redispersed rubber powder and rubber powder in a ratio of 1:0.5, add a small amount of water, and stir well to form a uniform rubber redispersed rubber powder mixture;
[0077] Step 3: slowly add the rubber redispersed rubber powder mixture prepared in step 2 to the cement slurry prepared in step 1, and stir evenly to make it fully mixed, and then add an appropriate amount of water reducing agent or retarder;
[0078] Step 4: Finally, pour the treated mixed material into the mold, compact and vibrate it with a press, use a vacuum degassing device to degas the slurry in the mold to remove bubbles and improve the density of the material, harden the treated composite material, wait for 36 hours for it to fully solidify, take out the solidified composite material, trim and polish it to make its surface smooth;
[0079] Step 5: After processing, the material is subjected to performance tests including damping performance, hardness, tensile strength, bending strength, and durability to ensure that it meets the requirements.
[0080] The specific contents of the materials in step one are as follows:
[0081] The redispersible rubber powder is polyvinyl alcohol or polyacrylate, used as a binder, and is used to improve the strength and toughness of the material;
[0082] Rubber powder is styrene-butadiene rubber or polychloroprene rubber, which is the core of the damping material and provides the damping performance of the material. Rubber powder is used to reduce vibration energy;
[0083] High-grade cement is P.O42.5, and high-grade cement is used to provide strength and hardness to the material;
[0084] Silica fume is fly ash or slag powder. As an admixture of high-grade cement, silica fume is used to improve the crack resistance and durability of the material;
[0085] The particle size range of quartz sand is 0.5mm. Quartz sand is used to improve the strength and durability of materials.
[0086] In step 1, the specific steps of mixing high-grade cement, silica fume and quartz sand are as follows:
[0087] Step 1: First, dry-mix cement and silica fume, then add water to mix, then add quartz sand and stir until uniform;
[0088] Step 2: Use a forced mixer to fully mix cement, silica fume, quartz sand and water to ensure the uniformity and fluidity of the concrete. The mixing time is 3 minutes.
[0089] Preferably, in step 2, the specific steps of mixing the redispersed rubber powder and the rubber powder are as follows:
[0090] Step 1: Make sure the operating environment is clean and has adequate ventilation, and prepare to disperse the rubber powder and rubber powder;
[0091] Step 2: Dry and grind the damp or agglomerated powder. After the powder is kept dry and dispersed, use accurate weighing equipment to weigh the required redispersed rubber powder and rubber powder for later use.
[0092] Step 3: Place the pre-treated redispersed rubber powder and rubber powder into a blender or mixing tank, start the mixing equipment, stir at a low speed first, and gradually increase the speed to ensure that the powders are evenly mixed. After mixing, take samples for quality inspection.
[0093] In step 4, the specific steps of the vacuum degassing equipment are:
[0094] Step 1: Check whether the vacuum degassing equipment is intact and ensure that it is in normal working condition. Then pour the mixed slurry into the mold and place the mold on the workbench of the vacuum degassing equipment to ensure that the mold is sealed and connected to the equipment.
[0095] Step 2: Then start the vacuum degassing equipment, start vacuuming, observe the vacuum gauge, and stop vacuuming when the vacuum reaches the set value. The vacuum is at 0.1 bar;
[0096] Step 3: Keep the slurry in vacuum for a certain period of time to allow the bubbles in the slurry to fully escape. The degassing time is usually 30 minutes. Observe the surface of the slurry. When no more bubbles emerge, it means that the degassing process is completed.
[0097] Step 4: Finally, slowly release the vacuum to avoid bubbles in the slurry due to pressure changes. After degassing is completed, remove the mold from the vacuum degassing equipment.
[0098] In step 5, the performance test specifically includes the following:
[0099] Damping performance test: Use a dynamic mechanical analyzer and a vibration table to simulate the performance of polymer damping composite materials in a vibration environment. Analyze the dynamic mechanical properties of the material by applying dynamic loading and measuring the response. Measure the damping performance of polymer damping composite materials at different frequencies and temperatures, and determine the damping peak, damping bandwidth and damping temperature key parameters of the composite materials.
[0100] Hardness performance test: Use a hardness tester to measure the hardness of the material, which reflects the hardness and compressive resistance of the material. Place the hardness tester on the sample surface, apply a certain load, and measure the diameter or depth of the impression to calculate the hardness value of the material;
[0101] Bending strength and tensile strength performance test: Use a universal material testing machine to measure the tensile, compression, bending and shear mechanical properties of the material. Use a fixture to fix the sample on the testing machine, apply mechanical loading and measure the stress-strain curve of the material;
[0102] Durability performance test: A fatigue testing machine is used to evaluate the durability of materials under cyclic loads or vibration loading. Continuous loads or vibrations are applied and the deformation and damage of the material during repeated loading are observed.
[0103] Performance test table:
[0104] Test items Test Method Typical values or evaluation criteria Damping Dynamic Mechanical Analyzer and Vibration Table 97.9% damping ratio hardness Hardness Tester Maintain 97% of initial strength Flexural strength and tensile strength Universal material testing machine 12MPa and 15MPa Durability Fatigue testing machine Maintain 98.78% of initial strength
[0105] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a polymer damping composite material, characterized in that: The specific steps include: Step 1: First prepare the following raw materials by mass percentage: 5% to 15% redispersed rubber powder, 5% to 15% rubber powder, 30% to 40% high-grade cement, 5% to 15% silica fume and 15% to 20% quartz sand, then take high-grade cement: silica fume: quartz sand in a ratio of 1:0.3:(0.5-1.5) and mix them evenly with a mixer, add appropriate amount of water and stir well to make cement slurry; Step 2: Weigh and mix the redispersed rubber powder and rubber powder in a ratio of 1:0.5, add a small amount of water, and stir well to form a uniform rubber redispersed rubber powder mixture; Step 3: slowly add the rubber redispersed rubber powder mixture prepared in step 2 to the cement slurry prepared in step 1, and stir evenly to make it fully mixed, and then add an appropriate amount of water reducing agent or retarder; Step 4: Finally, pour the treated mixed material into the mold, compact and vibrate it with a press, use a vacuum degassing device to degas the slurry in the mold to remove bubbles and improve the density of the material, harden the treated composite material, wait for 24 to 36 hours for it to fully solidify, take out the solidified composite material, trim and polish it to make its surface smooth; Step 5: After processing, the material is subjected to performance tests including damping performance, hardness, tensile strength, bending strength, and durability to ensure that it meets the requirements.
2. The method for preparing a polymer damping composite material according to claim 1, characterized in that: The specific contents of the materials in step 1 are as follows: The redispersed rubber powder is polyvinyl alcohol or polyacrylate, used as a binder, and the redispersed rubber powder is used to improve the strength and toughness of the material; The rubber powder is styrene-butadiene rubber or polychloroprene rubber, which is the core of the damping material and provides the damping performance of the material. The rubber powder is used to reduce vibration energy; The high-grade cement is P.O42.5, and the high-grade cement is used to provide strength and hardness of the material; The silica fume is fly ash or slag powder, which is used as an admixture of high-grade cement to improve the crack resistance and durability of the material; The quartz sand has a particle size range of 0.1 to 0.5 mm and is used to improve the strength and durability of the material.
3. The method for preparing a polymer damping composite material according to claim 1, characterized in that: In step 1, the specific steps of mixing high-grade cement, silica fume and quartz sand are as follows: Step 1: First, dry-mix cement and silica fume, then add water to mix, then add quartz sand and stir until uniform; Step 2: Use a forced mixer to fully mix cement, silica fume, quartz sand and water to ensure the uniformity and fluidity of the concrete. The mixing time is 2 to 3 minutes.
4. The method for preparing a polymer damping composite material according to claim 1, characterized in that: In the step 2, the specific steps of mixing the redispersed rubber powder and the rubber powder are as follows: Step 1: Make sure the operating environment is clean and has adequate ventilation, and prepare to disperse the rubber powder and rubber powder; Step 2: Dry and grind the damp or agglomerated powder. After the powder is kept dry and dispersed, use accurate weighing equipment to weigh the required redispersed rubber powder and rubber powder for later use. Step 3: Place the pre-treated redispersed rubber powder and rubber powder into a blender or mixing tank, start the mixing equipment, stir at a low speed first, and gradually increase the speed to ensure that the powders are evenly mixed. After mixing, take samples for quality inspection.
5. The method for preparing a polymer damping composite material according to claim 1, characterized in that: In the step 4, the method of using a vacuum degassing device to degas the slurry in the mold includes the following specific steps: Step 1: Check whether the vacuum degassing equipment is intact and ensure that it is in normal working condition. Then pour the mixed slurry into the mold and place the mold on the workbench of the vacuum degassing equipment to ensure that the mold is sealed and connected to the equipment. Step 2: Then start the vacuum degassing equipment, start vacuuming, observe the vacuum gauge, and stop vacuuming when the vacuum reaches the set value. The vacuum is between 0.05 and 0.1 bar. Step 3: Keep the slurry in vacuum for a certain period of time to allow the bubbles in the slurry to fully escape. The degassing time is usually 10 to 30 minutes. Observe the surface of the slurry. When no more bubbles emerge, the degassing process is completed. Step 4: Finally, slowly release the vacuum to avoid bubbles in the slurry due to pressure changes. After degassing is completed, remove the mold from the vacuum degassing equipment.
6. The method for preparing a polymer damping composite material according to claim 1, characterized in that: In step 5, the performance test specifically includes the following contents: Damping performance test: Use a dynamic mechanical analyzer and a vibration table to simulate the performance of polymer damping composite materials in a vibration environment. Analyze the dynamic mechanical properties of the material by applying dynamic loading and measuring the response. Measure the damping performance of polymer damping composite materials at different frequencies and temperatures, and determine the damping peak, damping bandwidth and damping temperature key parameters of the composite materials. Hardness performance test: Use a hardness tester to measure the hardness of the material, which reflects the hardness and compressive resistance of the material. Place the hardness tester on the sample surface, apply a certain load, and measure the diameter or depth of the impression to calculate the hardness value of the material; Bending strength and tensile strength performance test: Use a universal material testing machine to measure the tensile, compression, bending and shear mechanical properties of the material. Use a fixture to fix the sample on the testing machine, apply mechanical loading and measure the stress-strain curve of the material; Durability performance test: A fatigue testing machine is used to evaluate the durability of materials under cyclic loads or vibration loading. Continuous loads or vibrations are applied and the deformation and damage of the material during repeated loading are observed.