Recycled concrete aggregate semi-rigid base material in seasonal frozen region and preparation method and application of recycled concrete aggregate semi-rigid base material

By using recycled concrete aggregate materials with specific proportions in road projects in the frozen-freezing area, the structural cracks and durability problems of traditional semi-rigid base materials are solved under the freeze-thaw cycle, and the mechanical properties and anti-freeze-thaw deformation properties of the materials are achieved. The improvement of water stability performance extends the service life of the road and reduces environmental pollution.

CN118930178APending Publication Date: 2024-11-12CCCC THIRD HIGHWAY ENG CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411094743.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The application of traditional semi-rigid base materials in the freezing area has problems such as structural cracks, reduced durability and increased maintenance costs caused by freeze-thaw cycles.

Method used

Recycled concrete aggregate materials, including recycled coarse aggregate, recycled fine aggregate, cement, hydrated lime, fly ash, slag, alkali triggers, phosphogypsum and MoS2 nanomodified graphene oxide, through specific raw material ratios and Process processing improves the mechanical properties of the material, anti-freeze-thaw deformation and water stability.

Benefits of technology

It significantly improves the mechanical properties, anti-freeze-thaw deformation and durability of the semi-rigid base material of recycled concrete aggregate in the quaternary freezing area, reduces microcrack propagation under the freeze-thaw cycle, extends the service life of the road, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987564300000051
    Figure BDA0004987564300000051
  • Figure BDA0004987564300000061
    Figure BDA0004987564300000061
  • Figure BDA0004987564300000071
    Figure BDA0004987564300000071
Patent Text Reader

Abstract

The invention relates to the technical field of road engineering. The invention discloses a recycled concrete aggregate semi-rigid base material in a seasonal frozen region as well as a preparation method and application thereof. The semi-rigid base material is prepared from the following raw materials: recycled coarse aggregate, recycled fine aggregate, cement, slaked lime, fly ash, slag, an alkali activator, phosphogypsum, MoS2 nano-modified graphene oxide and water. The preparation method comprises the following steps: mixing and dispersing MoS2 nano-modified graphene oxide and water to prepare a premix; mixing the cement, the slaked lime, the fly ash, the slag, the alkali activator and the ardealite to prepare a mixture; and adding the mixture into the recycled coarse aggregate and the recycled fine aggregate, stirring, adding the premix, and stirring to obtain the concrete. The invention further discloses application of the semi-rigid base material in road engineering in seasonal frozen areas. The prepared recycled concrete aggregate semi-rigid base material in the seasonal frozen region is excellent in mechanical property, freeze-thaw deformation resistance, durability and water stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of road engineering, and in particular to a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas, and a preparation method and application thereof. Background Art

[0002] With the acceleration of global infrastructure construction, especially in the field of highway engineering, the demand for sand and gravel resources as basic building materials continues to grow, and it has gradually become a strategic mineral from ordinary raw materials in the construction industry to key raw materials related to national economic development. The continuous rise in sand and gravel prices has prompted the construction industry to explore more efficient and environmentally friendly solutions. In this situation, the application value of recycled concrete aggregate as a recyclable resource cannot be ignored, especially in seasonally frozen areas with harsh environmental conditions.

[0003] At present, semi-rigid base is commonly used in road construction in seasonally frozen areas. This base structure is formed by stabilizing soil or aggregate with inorganic binders. It has certain plate properties, bending strength and its own water stability, balancing the hardness of the rigid base and the toughness of the flexible base, ensuring the stability and durability of the road structure.

[0004] However, the application of traditional semi-rigid base materials in seasonally frozen areas has some limitations, mainly reflected in: the temperature fluctuations in seasonally frozen areas are large, and semi-rigid base materials are prone to frost heave and melt shrinkage after repeated freeze-thaw cycles, resulting in cracks inside the base and reducing the structural integrity of the base; frost heave caused by snowmelt and rainwater infiltration aggravates the damage to the base and affects durability. These problems not only shorten the service life of the road, but also increase maintenance costs.

[0005] Therefore, there is an urgent need to develop a semi-rigid base material for recycled concrete aggregate in seasonally frozen areas with excellent mechanical properties, freeze-thaw deformation resistance, durability and water stability. Summary of the invention

[0006] In order to solve at least one of the above technical problems, a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas with excellent mechanical properties, anti-freeze-thaw deformation properties, durability and water stability is developed. The present application provides a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas and a preparation method and application thereof.

[0007] On the one hand, the semi-rigid base material of recycled concrete aggregate for seasonally frozen areas provided in the present application comprises, by weight, 50 to 70 parts of recycled coarse aggregate, 20 to 40 parts of recycled fine aggregate, 5 to 15 parts of cement, 5 to 10 parts of slaked lime, 5 to 15 parts of fly ash, 5 to 10 parts of slag, 0.1 to 3 parts of alkali activator, 1 to 5 parts of phosphogypsum, 0.1 to 1 part of MoS2 nano-modified graphene oxide, and 5 to 7 parts of water.

[0008] By adopting the above technical scheme, the application adopts specific raw materials and proportions to obtain a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas with good mechanical properties, good freeze-thaw deformation resistance, excellent durability and water stability. The application adds recycled coarse aggregate and recycled fine aggregate to recycle construction waste, reduce the consumption of natural resources, and reduce environmental pollution. The addition of slaked lime helps to activate the active substances in fly ash and slag, and enhance the overall water stability and freeze-thaw resistance of the material.

[0009] The application adds MoS2 nano-modified graphene oxide, which can effectively improve the interfacial bonding strength of the material, reduce the expansion of microcracks under freeze-thaw cycles, and enhance the mechanical properties and deformation resistance of the material. At the same time, it can also improve the material's anti-freeze-thaw ability, reduce the expansion stress caused by freezing, and protect the base from damage by freeze-thaw cycles.

[0010] Optionally, the raw material composition includes, by weight: 55-65 parts of recycled coarse aggregate, 25-35 parts of recycled fine aggregate, 8-12 parts of cement, 7-8 parts of slaked lime, 8-12 parts of fly ash, 7-8 parts of slag, 1-2 parts of alkali activator, 2-4 parts of phosphogypsum, 0.2-0.8 parts of MoS2 nano-modified graphene oxide, and 5.5-6.5 parts of water.

[0011] Optionally, the raw material composition includes, by weight: 60 parts of recycled coarse aggregate, 30 parts of recycled fine aggregate, 10 parts of cement, 7.5 parts of slaked lime, 10 parts of fly ash, 7.5 parts of slag, 1.5 parts of alkali activator, 3 parts of phosphogypsum, 0.5 parts of MoS2 nano-modified graphene oxide, and 6 parts of water.

[0012] Optionally, the recycled coarse aggregate is formed by crushing, sorting, magnetic separation, strengthening and screening of waste concrete or waste bricks and stones; the recycled fine aggregate is formed by crushing, sorting, magnetic separation, strengthening and screening of waste concrete.

[0013] By adopting the above technical solution, this application uses waste concrete or waste masonry as the source of recycled aggregate, which can effectively reduce the landfill volume of construction waste and reduce the burden on the environment. It promotes the recycling of resources and conforms to the concept of sustainable development. The use of recycled aggregates also reduces dependence on natural aggregates and protects the natural environment and resources. By processing waste concrete and masonry through crushing, sorting, magnetic separation, strengthening and screening processes, the stability of recycled aggregates can be improved, the durability of recycled aggregates can be improved, and the service life of semi-rigid base material structures can be extended.

[0014] Optionally, the recycled coarse aggregate is composed of three-graded particle sizes of 5-10 mm, 10-20 mm and 20-30 mm, wherein the weight ratio of the recycled coarse aggregate with a particle size of 5-10 mm, a particle size of 10-20 mm and a particle size of 20-30 mm is 30-40:40-50:10-30.

[0015] By adopting the above technical solution, the appropriate gradation of the recycled coarse aggregate in the present application can improve the permeability of the semi-rigid base material and enhance its anti-erosion ability.

[0016] Optionally, the average particle size of the recycled fine aggregate is 0.15 to 4.75 mm.

[0017] By adopting the above technical solution, the smaller average particle size of the recycled fine aggregate of the present application can be well filled in the gaps of the coarse aggregate, increasing the density of the semi-rigid base material, thereby improving the impermeability and durability of the semi-rigid base material.

[0018] Optionally, the cement is ordinary Portland cement.

[0019] By adopting the above technical solution, the ordinary Portland cement used in this application has wide applicability, good hydration characteristics, and good compatibility with other raw materials.

[0020] Optionally, the weight ratio of the cement, slag and phosphogypsum is 3 to 4:2 to 3:1.

[0021] By adopting the above technical solution, the weight ratio of cement, slag and phosphogypsum in the present application can enhance the freeze-thaw resistance of the semi-rigid base material and improve its durability.

[0022] Optionally, the alkaline activator is selected from at least one of sodium hydroxide, hydrotalcite and aluminum sulfate.

[0023] Optionally, the alkaline activator is hydrotalcite and aluminum sulfate in a weight ratio of 1:1 to 2.

[0024] By adopting the above technical solutions, hydrotalcite can slowly release alkaline ions and continuously stimulate the active substances in the semi-rigid base material, which helps to improve the long-term strength and stability of the semi-rigid base material. In seasonally frozen areas, the slow-release effect of hydrotalcite helps the material maintain good performance in multiple freeze-thaw cycles. The addition of aluminum sulfate can promote the interfacial bonding between aggregate and cement matrix, reduce the generation of microcracks, and enhance the material's freeze-thaw resistance and durability. The combined effect of hydrotalcite and aluminum sulfate can effectively improve bonding performance, reduce microcracks, and enhance overall mechanical properties and durability.

[0025] Optionally, the preparation method of the MoS2 nano-modified graphene oxide is: dispersing graphene oxide in a solvent, adding MoS2 nanoparticles, adding a surfactant, stirring and mixing, centrifuging, filtering, drying, calcining at 400 to 800° C. for 4 to 10 hours, cooling, and obtaining MoS2 nano-modified graphene oxide; Among them, the weight ratio of graphene oxide and MoS2 nanoparticles is 1-3:1; the weight ratio of graphene oxide and solvent is 1:5-10; and the added amount of surfactant is 0.1-5%.

[0026] By adopting the above technical solution, MoS2 nano-modified graphene oxide can significantly enhance the interfacial adhesion, improve the mechanical properties and crack resistance of semi-rigid base materials, and also help improve the density and water stability of concrete.

[0027] Optionally, the solvent is selected from one of ethanol, water and N-methylpyrrolidone.

[0028] Optionally, the surfactant is selected from one of sodium dodecyl sulfate and hexadecyltrimethylammonium bromide.

[0029] In a second aspect, the present application provides a method for preparing the above-mentioned semi-rigid base material of recycled concrete aggregate in seasonally frozen areas, comprising the following steps: S1, mixing and dispersing the MoS2 nano-modified graphene oxide with water to prepare a premix; S2, mixing the cement, slaked lime, fly ash, slag, alkali activator and phosphogypsum to prepare a mixture; S3, adding the mixed material to the recycled coarse aggregate and recycled fine aggregate, stirring, adding the premix, stirring, and obtaining a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas.

[0030] By adopting the above technical solution, the preparation method adopted in the present application is simple and convenient to operate, ensuring the uniform dispersion of the material, which is beneficial to improving the mechanical properties and durability of the material.

[0031] On the third aspect, the present application provides the application of the above-mentioned semi-rigid base material of recycled concrete aggregate in seasonally frozen areas in road projects in seasonally frozen areas.

[0032] Optionally, the construction method of the above-mentioned semi-rigid base material of recycled concrete aggregate in seasonally frozen areas is: Step 1: Clean the surface of the base layer to ensure that there is no debris or loose soil, and the ground is flat and solid; Step 2: Spread and mix the semi-rigid base material of recycled concrete aggregate in the seasonally frozen area and roll it; Step 3: After rolling is completed, re-rolling is performed; Step 4: Cover with film and cure to form a semi-rigid base layer after solidification.

[0033] By adopting the above technical solutions, cleaning the surface of the base layer can ensure that the base layer is clean, flat and free of debris, providing a good bonding foundation for the newly laid semi-rigid base layer, and preventing local stress concentration caused by uneven base layer or debris, which affects the stability of the overall structure. Spreading and rolling make the material denser, ensure the tightness of the internal structure of the material, improve the bearing capacity and deformation resistance, and eliminate bubbles in the material, enhancing the continuity and uniformity of the material. Covering film can effectively maintain the humidity of the base layer, control the evaporation rate of water, create favorable conditions for cement hydration reaction, accelerate strength development, and avoid cracking caused by excessive water loss.

[0034] In summary, the present invention includes at least one of the following beneficial technical effects: 1. This application adopts specific raw materials and proportions to produce a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas with good mechanical properties, good resistance to freeze-thaw deformation, excellent durability and water stability.

[0035] 2. This application adds recycled coarse aggregate and recycled fine aggregate to recycle construction waste, reduce the consumption of natural resources, and reduce environmental pollution.

[0036] 3. The preparation method adopted in this application is simple and convenient to operate, which ensures the uniform dispersion of the material and is beneficial to improving the mechanical properties and durability of the material. DETAILED DESCRIPTION

[0037] The present application is further described in detail below in conjunction with embodiments.

[0038] The present application designs a semi-rigid base material of recycled concrete aggregate for seasonally frozen areas. The raw material composition thereof includes, by weight: 50-70 parts of recycled coarse aggregate, 20-40 parts of recycled fine aggregate, 5-15 parts of cement, 5-10 parts of slaked lime, 5-15 parts of fly ash, 5-10 parts of slag, 0.1-3 parts of alkali activator, 1-5 parts of phosphogypsum, 0.1-1 parts of MoS2 nano-modified graphene oxide, and 5-7 parts of water.

[0039] The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas of the present application is prepared by the following method, comprising the following steps: S1, mixing and dispersing the MoS2 nano-modified graphene oxide with water to prepare a premix; S2, mixing the cement, slaked lime, fly ash, slag, alkali activator and phosphogypsum to prepare a mixture; S3, adding the mixed material to the recycled coarse aggregate and recycled fine aggregate, stirring, adding the premix, stirring, and obtaining a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas.

[0040] The seasonally frozen zone recycled concrete aggregate semi-rigid base material of the present application can be used in seasonally frozen zone road projects.

[0041] The applicant has designed the technical solution of the present application to address the problem that the existing semi-rigid base in seasonally frozen areas is prone to cracks after repeated freeze-thaw cycles, and has poor freeze-thaw deformation resistance, durability and water stability.

[0042] The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas proposed in this application has excellent mechanical properties, anti-freeze-thaw deformation properties, durability and water stability.

[0043] The raw materials used in this application are as follows: Hydrated lime: Hubei Chengfeng Chemical Co., Ltd., purity: 99%.

[0044] Hydrotalcite: CAS: 12304-65-3.

[0045] Aluminum sulfate: CAS: 10043-01-3.

[0046] Phosphogypsum: Shandong Dongshun Gypsum Products Co., Ltd., item number: 01.

[0047] N-Methylpyrrolidone: CAS: 872-50-4.

[0048] Ammonium tetrathiomolybdate: CAS: 15060-55-6.

[0049] Sodium dodecyl sulfate: CAS: 151-21-3.

[0050] Hexadecyltrimethylammonium bromide: CAS: 57-09-0. Specific embodiments

[0051] The preparation method of the MoS2 nano-modified graphene oxide used in Examples 1 to 5 is as follows: ultrasonically dispersing graphene oxide in a solvent, adding MoS2 nanoparticles, adding a surfactant, stirring and mixing, centrifuging, filtering, drying, calcining at 600°C for 7h, and cooling naturally to obtain MoS2 nano-modified graphene oxide; The weight ratio of graphene oxide to MoS2 nanoparticles is 2:1; the weight ratio of graphene oxide to solvent is 1:10; the amount of surfactant added is 2%; The solvent is N-methylpyrrolidone; the surfactant is hexadecyltrimethylammonium bromide; The preparation of MoS2 nanoparticles is as follows: ammonium tetrathiomolybdate powder, deionized water and sodium dodecyl sulfate in a weight ratio of 1:25:0.5 are mixed, filtered, placed at 400°C for 6 hours, and cooled to room temperature to obtain MoS2 nanoparticles.

[0052] Embodiments 1 to 5 The specific raw material weight proportions of the semi-rigid base material of recycled concrete aggregate for seasonally frozen areas prepared in Examples 1 to 5 are shown in Table 1.

[0053] Table 1 The recycled coarse aggregate is made from waste concrete through crushing, sorting, magnetic separation, strengthening and screening processes; the recycled fine aggregate is made from waste concrete through crushing, sorting, magnetic separation, strengthening and screening processes; the recycled coarse aggregate is composed of three-graded particle sizes of 5-10mm, 10-20mm and 20-30mm, among which the weight ratio of recycled coarse aggregate with particle sizes of 5-10mm, 10-20mm and 20-30mm is 30:40:10; the average particle size of the recycled fine aggregate is 2.50mm; the cement is P·O52.5R ordinary Portland cement; the specific surface area of ​​the fly ash is 300m 2 / g; the specific surface area of ​​slag is 450m 2 / g; the weight percentage of oxygen in graphene oxide is 25%; the alkaline activator is aluminum sulfate; The preparation method of Example 1 comprises the following steps: S1, mixing and dispersing MoS2 nano-modified graphene oxide with water to prepare a premix; S2, mixing cement, slaked lime, fly ash, slag, alkali activator and phosphogypsum to prepare a mixture; S3, adding the recycled coarse aggregate and the recycled fine aggregate into the mixture, stirring, adding the premix, stirring, and obtaining the semi-rigid base material of recycled concrete aggregate in seasonally frozen areas.

[0054] The preparation methods of Examples 2 to 5 are consistent with that of Example 1.

[0055] The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas prepared in Examples 1 to 5 can be used in seasonally frozen area road projects. The specific construction method is as follows: Step 1: Clean the surface of the base layer to ensure that there is no debris or loose soil, and the ground is flat and solid; Step 2: Spread and mix the semi-rigid base material of recycled concrete aggregate in the seasonally frozen area and roll it; Step 3: After rolling is completed, re-rolling is performed; Step 4: Cover the film and cure it for 7 days to form a semi-rigid base after solidification.

[0056] Comparative Examples 1 to 4 Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that MoS2 nano-modified graphene oxide is not added in Comparative Example 1.

[0057] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, the MoS2 nano-modified graphene oxide is replaced with an equal amount of graphene oxide.

[0058] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that in Comparative Example 3, the MoS2 nano-modified graphene oxide is replaced with an equal amount of MoS2 nanoparticles.

[0059] Comparative Example 4 The difference between Comparative Example 4 and Example 3 is that Comparative Example 4 has no premixing step, and all raw materials are directly mixed. The specific preparation method is: recycled coarse aggregate, recycled fine aggregate, cement, slaked lime, fly ash, slag, alkali activator, phosphogypsum, MoS2 nano-modified graphene oxide and water are mixed and stirred to obtain a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas.

[0060] Experimental testing Test items and test methods According to T0805 in JTG 3441-2024 "Testing Procedures for Inorganic Binder Stabilized Materials for Highway Engineering", the unconfined compressive strength of semi-rigid base materials is tested; According to T0855 in JTG 3441-2024 "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering", the prepared semi-rigid base material is subjected to a temperature shrinkage test to detect the temperature shrinkage coefficient, thereby evaluating its anti-freeze-thaw deformation performance; According to T0865 of JTG 3441-2024 "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering", the prepared semi-rigid base material is subjected to fatigue test to detect fatigue life and thus evaluate its durability; According to T0805 in JTG 3441-2024 "Testing Procedure for Inorganic Binder Stabilized Materials for Highway Engineering", the specimens were saturated with water (immersed in water for 24 hours), and then the unconfined compressive strength of the semi-rigid base material was tested, and the saturated compressive strength ratio was calculated, which is (saturated strength / unsaturated strength) × 100%; The unconfined compressive strength, thermal shrinkage coefficient, fatigue life and saturated compressive strength ratio of the semi-rigid base materials of recycled concrete aggregates in seasonally frozen areas prepared in Examples 1 to 5 and Comparative Examples 1 to 4 were tested. The test results are shown in Table 2.

[0061] Table 2 From the test results in Table 1, it can be seen that the semi-rigid base material of recycled concrete aggregate in seasonally frozen areas prepared in Examples 1 to 5 has high unconfined compressive strength and good mechanical properties; low temperature shrinkage coefficient, good freeze-thaw deformation resistance; high fatigue life and good durability; high saturated compressive strength ratio and excellent water stability. Among them, the semi-rigid base material of recycled concrete aggregate in seasonally frozen areas prepared in Example 3 has the best mechanical properties, freeze-thaw deformation resistance, durability and water stability.

[0062] In Comparative Example 1, no MoS2 nano-modified graphene oxide was added, and the mechanical properties, freeze-thaw deformation resistance, durability and water stability of the semi-rigid base material of recycled concrete aggregate in seasonally frozen areas were significantly reduced. Therefore, the inventors speculate that MoS2 nano-modified graphene oxide can improve the interfacial bonding strength of the material, enhance the mechanical properties and freeze-thaw deformation resistance of the material, and can also improve the freeze-thaw resistance and durability of the material.

[0063] The mechanical properties, freeze-thaw deformation resistance, durability and water stability of the semi-rigid base materials of recycled concrete aggregate in seasonally frozen areas prepared in Comparative Examples 2 and 3 are all inferior to those in Example 3.

[0064] The mechanical properties and durability of the semi-rigid base material of recycled concrete aggregate in seasonally frozen areas prepared in Example 4 are reduced. The inventors speculate that one-step mixing cannot ensure uniform dispersion of the material, thus affecting the mechanical properties and durability of the material.

[0065] Embodiments 6 to 13 Example 6 The difference between Example 6 and Example 3 is that in Example 6, the weight ratio of the recycled coarse aggregate with a particle size of 5-10 mm, a particle size of 10-20 mm, and a particle size of 20-30 mm is 35:45:20.

[0066] Example 7 The difference between Example 7 and Example 3 is that in Example 7, the weight ratio of the recycled coarse aggregate with a particle size of 5-10 mm, a particle size of 10-20 mm, and a particle size of 20-30 mm is 40:50:30.

[0067] Example 8 The difference between Example 8 and Example 3 is that in Example 8, the weight ratio of cement, slag and phosphogypsum is 3:2:1, and the total weight of cement, slag and phosphogypsum remains unchanged.

[0068] Example 9 The difference between Example 9 and Example 3 is that in Example 9, the weight ratio of cement, slag and phosphogypsum is 4:3:1, and the total weight of cement, slag and phosphogypsum remains unchanged.

[0069] Example 10 The difference between Example 10 and Example 3 is that the base activator in Example 10 is hydrotalcite.

[0070] Embodiment 11 The difference between Example 11 and Example 3 is that the base activator in Example 11 is hydrotalcite and aluminum sulfate in a weight ratio of 1:1.

[0071] Example 12 The difference between Example 12 and Example 3 is that the base activator in Example 12 is hydrotalcite and aluminum sulfate in a weight ratio of 1:1.5.

[0072] Example 13 The difference between Example 13 and Example 3 is that the base activator in Example 13 is hydrotalcite and aluminum sulfate in a weight ratio of 1:2.

[0073] The unconfined compressive strength, thermal shrinkage coefficient, fatigue life and saturated compressive strength ratio of the semi-rigid base material of recycled concrete aggregate for seasonally frozen areas prepared in Examples 6 to 13 were tested. The test results are shown in Table 3.

[0074] Table 3 From the test results in Table 3, it can be seen that the proportions of recycled coarse aggregate in Examples 6 and 7 are different from those in Example 3, among which the comprehensive performance of the semi-rigid base material of recycled concrete aggregate for seasonally frozen areas prepared in Example 6 is the best.

[0075] The weight ratios of cement, slag and phosphogypsum in Examples 8 and 9 are different from those in Example 3. Among them, the comprehensive performance of the semi-rigid base material of recycled concrete aggregate for seasonally frozen areas prepared in Example 3 is the best.

[0076] The properties of the semi-rigid base material of recycled concrete aggregate for seasonally frozen areas prepared in Example 10 are similar to those in Example 3.

[0077] The comprehensive performance of the semi-rigid base material of recycled concrete aggregate for seasonally frozen areas prepared in Examples 11 to 13 is significantly higher than that of Example 3, among which the comprehensive performance of the semi-rigid base material of recycled concrete aggregate for seasonally frozen areas prepared in Example 12 is the best.

[0078] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. Semi-rigid base material of recycled concrete aggregate in seasonally frozen areas, characterized in that: The raw material composition includes, by weight: 50-70 parts of recycled coarse aggregate, 20-40 parts of recycled fine aggregate, 5-15 parts of cement, 5-10 parts of slaked lime, 5-15 parts of fly ash, 5-10 parts of slag, 0.1-3 parts of alkali activator, 1-5 parts of phosphogypsum, 0.1-1 parts of MoS2 nano-modified graphene oxide, and 5-7 parts of water.

2. The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas according to claim 1, characterized in that: The recycled coarse aggregate is made from waste concrete or waste bricks and stones through crushing, sorting, magnetic separation, strengthening and screening; the recycled fine aggregate is made from waste concrete through crushing, sorting, magnetic separation, strengthening and screening.

3. The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas according to claim 1, characterized in that: The recycled coarse aggregate is composed of three-graded particle sizes of 5-10 mm, 10-20 mm and 20-30 mm, wherein the weight ratio of the recycled coarse aggregate with a particle size of 5-10 mm, a particle size of 10-20 mm and a particle size of 20-30 mm is 30-40:40-50:10-30.

4. The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas according to claim 1, characterized in that: The average particle size of the recycled fine aggregate is 0.15-4.75 mm.

5. The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas according to claim 1, characterized in that: The weight ratio of the cement, slag and phosphogypsum is 3-4:2-3:

1.

6. The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas according to claim 1, characterized in that: The alkaline activator is selected from at least one of sodium hydroxide, hydrotalcite and aluminum sulfate.

7. The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas according to claim 1, characterized in that: The alkaline activator is hydrotalcite and aluminum sulfate in a weight ratio of 1:1-2.

8. The semi-rigid base material of recycled concrete aggregate in seasonally frozen areas according to claim 1, characterized in that: The preparation method of the MoS2 nano-modified graphene oxide is as follows: dispersing graphene oxide in a solvent, adding MoS2 nanoparticles, adding a surfactant, stirring and mixing, centrifuging, filtering, drying, calcining at 400-800°C for 4-10h, cooling, and obtaining MoS2 nano-modified graphene oxide; Among them, the weight ratio of graphene oxide and MoS2 nanoparticles is 1~3:1; the weight ratio of graphene oxide and solvent is 1:5~10; and the added amount of surfactant is 0.1~5%.

9. A method for preparing a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, mixing and dispersing the MoS2 nano-modified graphene oxide with water to prepare a premix; S2, mixing the cement, slaked lime, fly ash, slag, alkali activator and phosphogypsum to prepare a mixture; S3, adding the mixed material to the recycled coarse aggregate and recycled fine aggregate, stirring, adding the premix, stirring, and obtaining a semi-rigid base material of recycled concrete aggregate in seasonally frozen areas.

10. Use of the semi-rigid base material of recycled concrete aggregate in seasonally frozen areas according to any one of claims 1 to 8 in seasonally frozen area road engineering.

Citation Information

Cited By

  • Functional material for wet shotcrete and preparation method thereof