Anti-cleavage concrete containing modified polyester fibers and preparation method of anti-cleavage concrete

By using materials such as modified polyester fibers and modified clay in concrete, the crack resistance and anti-seepage performance of concrete is improved, the problem of insufficient performance of existing concrete is solved, and better mechanical and anti-seepage effects are achieved.

CN118930192AActive Publication Date: 2024-11-12珠海汇茂环保科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411217225.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

There are shortcomings in existing concrete in terms of anti-seepage and crack resistance, and further improvement is needed.

Method used

Using modified polyester fibers, the crack resistance with excellent anti-seepage properties is prepared by mixing and stirring silicate cement, quartz sand, aggregate, modified polyester fiber, hydrophobic agent, water reducing agent and water. Concrete. Modified polyester fibers are obtained by electron beam irradiation and nano-silica treatment. The aggregate is mixed with modified clay and limestone, and the hydrophobic agent is made of polycarboxylic acid water reducing agent or sodium lignin sulfonate.

Benefits of technology

The mechanical properties of concrete have been improved, while the anti-seepage performance has been significantly improved, ensuring product quality and quality, and having broader market prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005021883630000101
    Figure BDA0005021883630000101
  • Figure BDA0005021883630000111
    Figure BDA0005021883630000111
Patent Text Reader

Abstract

The invention relates to the technical field of concrete materials, in particular to anti-splitting concrete containing modified polyester fibers and a preparation method. The anti-splitting concrete containing the modified polyester fibers is prepared from the following raw materials in parts by weight: 100-120 parts of Portland cement, 10-14 parts of quartz sand, 20-30 parts of aggregate, 5-8 parts of the modified polyester fibers, 4-7 parts of a water repellent agent, 6-10 parts of a water reducing agent and 30-50 parts of water, portland cement, quartz sand, aggregate and modified polyester fibers are put into mixing equipment to be mixed and stirred, a mixture is obtained, a water repellent agent, a water reducing agent and water are fully mixed, then the mixture is added into the mixture, stirring and mixing are continued, discharging is conducted after material mixing is completed, and finally the finished anti-splitting concrete containing the modified polyester fibers is prepared. The anti-cleavage concrete containing modified polyester fibers prepared by the invention not only has better mechanical properties, but also has excellent anti-seepage performance, and the quality of the anti-cleavage concrete is effectively ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete materials, in particular to a modified polyester fiber-containing anti-splitting concrete and a preparation method thereof. Background Art

[0002] Concrete is an artificial stone made by mixing and curing cementitious materials, aggregates, water, etc. in a certain proportion. It has become the most widely used building material in the construction industry because of its wide source of raw materials, low price, simple production process, and good mechanical properties and durability.

[0003] In the patent document with application number "CN202010911918.7" and titled "A C35 basalt fiber concrete for abutments and its preparation method", it is recorded that "It is characterized by: in parts by weight, comprising 430-450 parts of cementitious materials, 4 parts of basalt fibers, 1790-1800 parts of aggregates, 7-8 parts of water reducers, and 150-170 parts of water; wherein the cementitious materials are composed of 2803-00 parts of cement, 60-70 parts of fly ash and 70-90 parts of slag powder, and the aggregates are composed of coarse aggregates and fine aggregates. The C35 basalt fiber concrete for abutments prepared by the present invention has a 28d compressive strength ≥35.0MPa, a 28d flexural strength ≥5.0MPa, a 28d splitting strength ≥3.0MPa, a 28d elastic modulus ≥30GPa, and a crack resistance grade of L-Ⅲ".

[0004] Although the concrete produced by the above patent document has advantages such as excellent mechanical properties, its own anti-seepage performance and anti-splitting performance are relatively insufficient and still need to be further improved. Based on this, the present invention provides a modified polyester fiber anti-splitting concrete and a preparation method to solve the above technical problems. Summary of the invention

[0005] The purpose of the present invention is to provide a modified polyester fiber-containing splitting-resistant concrete and a preparation method. The prepared modified polyester fiber-containing splitting-resistant concrete not only has good mechanical properties, but also has excellent anti-seepage performance, effectively ensuring its quality.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The first aspect of the present invention provides a modified polyester fiber-containing anti-splitting concrete, which is composed of the following raw materials in parts by weight: 100 to 120 parts of silicate cement, 10 to 14 parts of quartz sand, 20 to 30 parts of aggregate, 5 to 8 parts of modified polyester fibers, 4 to 7 parts of hydrophobic agent, 6 to 10 parts of water reducer and 30 to 50 parts of water.

[0008] The present invention is further configured as follows: the aggregate is formed by mixing modified clay and limestone in a mass ratio of 1:1.8 to 2.1.

[0009] The present invention is further configured as follows: the silicate cement is ordinary silicate cement P·O 42.5.

[0010] The present invention is further configured as follows: the preparation process of the modified clay is as follows:

[0011] Place the clay in a resistance furnace, heat it to 650-700°C at a heating rate of 8-10°C / min, and keep it at this temperature for 240-260min;

[0012] Then, the temperature is raised to 760-780°C at a heating rate of 4-6°C / min, and kept at this temperature for 100-120 minutes. After natural cooling, the mixture is placed in a pulverizing device and pulverized to 0.2-2.2 mm to obtain a powder.

[0013] The nano-silicon dioxide is ultrasonically dispersed in deionized water at a dosage ratio of 0.12 to 0.45 g / mL for 20 to 30 minutes to obtain a prepared solution;

[0014] The powder is placed in the prepared solution at a dosage ratio of 0.05-0.25 g / mL, and treated at 120-140 r / min for 30-36 hours. After filtration, it is dried at 70-80° C. to constant weight to obtain modified clay.

[0015] The present invention is further configured as follows: the preparation process of the modified polyester fiber is as follows:

[0016] Taking polytetrafluoroethylene fiber, and subjecting it to electron beam irradiation to obtain pretreated polytetrafluoroethylene fiber;

[0017] The silane coupling agent KH560 is placed in an ethanol aqueous solution with a concentration of 80-84% at a mass ratio of 0.65-0.75:1, stirred at 120-240 r / min for 10-14 min, and then nano-silicon dioxide is added thereto, and stirring is continued for 70-80 min;

[0018] Then, the pretreated polytetrafluoroethylene fiber is added thereto, and ultrasonic treatment is performed for 40 to 50 minutes. After filtration, the fiber is washed with anhydrous ethanol and deionized water for 2 to 4 times respectively, and dried at a temperature of 70 to 80° C. for 14 to 16 hours to obtain the modified polyester fiber.

[0019] The present invention is further configured as follows: the irradiation dose of the electron beam irradiation is 200 to 300 kGy, and the irradiation time is 10 to 12 s.

[0020] The present invention is further configured as follows: the addition amount of the nano silicon dioxide is 1.2-1.4% of the mass of the ethanol aqueous solution.

[0021] The present invention is further configured as follows: the addition amount of the pretreated polytetrafluoroethylene fiber is 4.3-6.3% of the mass of the ethanol aqueous solution.

[0022] The present invention is further configured as follows: the water reducer is selected from any one of a polycarboxylate water reducer and a sodium lignin sulfonate water reducer.

[0023] The second aspect of the present invention: also provides a method for preparing the above-mentioned anti-splitting concrete containing modified polyester fiber, comprising the following steps:

[0024] Step 1, accurately weighing silicate cement, quartz sand, aggregate, modified polyester fiber, hydrophobic agent, water reducing agent and water, and putting silicate cement, quartz sand, aggregate and modified polyester fiber into a mixing device for mixing and stirring to obtain a mixture;

[0025] Step 2: After the hydrophobic agent, water reducing agent and water are fully mixed, the mixture is added thereto, and the stirring and mixing is continued for 10 to 15 minutes. After the mixing is completed, the material is discharged to finally obtain a finished product of anti-splitting concrete containing modified polyester fiber.

[0026] The present invention is further configured as follows: in step 1, the rotation speed of the mixing equipment is 120 to 320 r / min, and the mixing time is 20 to 30 min.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] In the present invention, silicate cement, quartz sand, aggregate, modified polyester fiber, hydrophobic agent, water reducing agent and water are used as raw materials. The silicate cement, quartz sand, aggregate and modified polyester fiber are put into a mixing device for mixing and stirring to obtain a mixture. The hydrophobic agent, water reducing agent and water are fully mixed, and then the mixture is added thereto, and the mixing is continued. After the mixing is completed, the material is discharged to finally obtain a finished product of anti-split concrete containing modified polyester fiber. The anti-split concrete containing modified polyester fiber prepared by the present invention not only has good mechanical properties, but also has excellent anti-seepage performance, which effectively guarantees its quality. The anti-split concrete containing modified polyester fiber and the preparation method provided by the present invention have a broader market prospect and are more suitable for promotion. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] The present embodiment provides a modified polyester fiber-containing anti-splitting concrete, which is composed of the following raw materials in parts by weight: 100 parts of Portland cement, 10 parts of quartz sand, 20 parts of aggregate, 5 parts of modified polyester fiber, 4 parts of hydrophobic agent, 6 parts of water reducing agent and 30 parts of water.

[0032] In this embodiment, it should be noted that the silicate cement is ordinary silicate cement P·O42.5, which is purchased from Hunan Xindingli New Material Technology Co., Ltd.

[0033] Among them, the aggregate is a mixture of modified clay and limestone in a mass ratio of 1:1.8.

[0034] Further, the preparation process of modified clay is as follows:

[0035] The clay was placed in a resistance furnace, heated to 650°C at a heating rate of 8°C / min, and kept at this temperature for 240 min;

[0036] Then the temperature was raised to 760°C at a heating rate of 4°C / min and kept at that temperature for 100 minutes. After natural cooling, the mixture was placed in a pulverizing device and pulverized to 0.2 mm to obtain a powder.

[0037] The nano-silicon dioxide was ultrasonically dispersed in deionized water at a dosage of 0.12 g / mL for 20 min to obtain a prepared solution;

[0038] The powder was placed in the prepared solution at a dosage ratio of 0.05 g / mL and treated at 120 r / min for 30 h. After filtration, it was dried at 70° C. to constant weight to obtain modified clay.

[0039] In this embodiment, it should be noted that limestone was purchased from Shenyang Elepox Chemical Co., Ltd., clay was purchased from Shijiazhuang Fengming Mineral Products Co., Ltd., and nano-silicon dioxide was purchased from Aladdin Reagent (Shanghai) Co., Ltd.

[0040] Among them, the preparation process of modified polyester fiber is as follows:

[0041] Taking polytetrafluoroethylene fiber, and subjecting it to electron beam irradiation to obtain pretreated polytetrafluoroethylene fiber;

[0042] The silane coupling agent KH560 was placed in an 80% ethanol aqueous solution at a mass ratio of 0.65:1, stirred at 120 r / min for 10 min, and then nano-silicon dioxide was added thereto, and stirring was continued for 70 min;

[0043] Then, the pretreated polytetrafluoroethylene fiber was added thereto, and ultrasonic treatment was performed for 40 minutes. After filtration, the fiber was washed twice with anhydrous ethanol and deionized water respectively, and dried at 70° C. for 14 hours to obtain modified polyester fiber.

[0044] Furthermore, the irradiation dose of the electron beam irradiation is 20 kGy, and the irradiation time is 10 s.

[0045] In addition, the added amount of nano-silica is 1.2% of the mass of the ethanol aqueous solution.

[0046] The addition amount of the pretreated polytetrafluoroethylene fiber is 4.3% of the mass of the ethanol aqueous solution.

[0047] Among them, the water reducer is polycarboxylic acid water reducer.

[0048] In this embodiment, it should be noted that the polycarboxylate water reducer was purchased from Wuhan Runxingyuan Technology Co., Ltd.

[0049] In addition, this embodiment also provides a method for preparing the above-mentioned anti-splitting concrete containing modified polyester fibers, comprising the following steps:

[0050] Step 1: Accurately weigh silicate cement, quartz sand, aggregate, modified polyester fiber, hydrophobic agent, water reducing agent and water, and put silicate cement, quartz sand, aggregate and modified polyester fiber into a mixing device for mixing and stirring to obtain a mixture.

[0051] Among them, the rotation speed of the mixing equipment is 120r / min, and the mixing time is 20min.

[0052] Step 2: After the hydrophobic agent, water reducing agent and water are fully mixed, the mixture is added thereto, and the stirring and mixing is continued for 10 minutes. After the mixing is completed, the material is discharged, and finally a finished product of anti-split concrete containing modified polyester fiber is obtained.

[0053] Example 2

[0054] The preparation method of the modified polyester fiber-containing anti-split concrete provided in this embodiment is basically the same as that in Embodiment 1, except that: the specific raw material composition and the specific preparation method of the modified polyester fiber-containing anti-split concrete in this embodiment are different; the specific raw material composition and the specific preparation method of the modified polyester fiber-containing anti-split concrete in this embodiment are as follows:

[0055] A modified polyester fiber-containing anti-splitting concrete is composed of the following raw materials in parts by weight: 110 parts of Portland cement, 12 parts of quartz sand, 25 parts of aggregate, 6 parts of modified polyester fiber, 6 parts of hydrophobic agent, 8 parts of water reducing agent and 40 parts of water.

[0056] In this embodiment, it should be noted that the silicate cement is ordinary silicate cement P·O42.5, which is purchased from Hunan Xindingli New Material Technology Co., Ltd.

[0057] Among them, the aggregate is a mixture of modified clay and limestone in a mass ratio of 1:1.9.

[0058] Further, the preparation process of modified clay is as follows:

[0059] The clay was placed in a resistance furnace, heated to 675°C at a heating rate of 9°C / min, and kept at this temperature for 250 min;

[0060] Then the temperature was raised to 770°C at a heating rate of 5°C / min and kept at that temperature for 110min. After natural cooling, the mixture was placed in a pulverizing device and pulverized to 1.2mm to obtain a powder.

[0061] The nano-silicon dioxide was ultrasonically dispersed in deionized water at a dosage of 0.32 g / mL for 25 min to obtain a prepared solution;

[0062] The powder was placed in the prepared solution at a dosage ratio of 0.15 g / mL and treated at 130 r / min for 33 h. After filtration, it was dried at 75° C. to constant weight to obtain modified clay.

[0063] In this embodiment, it should be noted that limestone was purchased from Shenyang Elepox Chemical Co., Ltd., clay was purchased from Shijiazhuang Fengming Mineral Products Co., Ltd., and nano-silicon dioxide was purchased from Aladdin Reagent (Shanghai) Co., Ltd.

[0064] Among them, the preparation process of modified polyester fiber is as follows:

[0065] Taking polytetrafluoroethylene fiber, and subjecting it to electron beam irradiation to obtain pretreated polytetrafluoroethylene fiber;

[0066] The silane coupling agent KH560 was placed in an ethanol aqueous solution with a concentration of 82% at a mass ratio of 0.7:1, stirred at 180 r / min for 12 min, and then nano-silicon dioxide was added thereto, and stirring was continued for 75 min;

[0067] Then, the pretreated polytetrafluoroethylene fiber was added thereto, and ultrasonic treatment was performed for 45 minutes. After filtration, the fiber was washed with anhydrous ethanol and deionized water for three times respectively, and dried at a temperature of 75° C. for 15 hours to obtain the modified polyester fiber.

[0068] Furthermore, the irradiation dose of the electron beam irradiation is 250 kGy, and the irradiation time is 11 s.

[0069] In addition, the added amount of nano-silica is 1.3% of the mass of the ethanol aqueous solution.

[0070] The addition amount of the pretreated polytetrafluoroethylene fiber is 5.3% of the mass of the ethanol aqueous solution.

[0071] Among them, the water reducer is lignin sulfonate sodium salt water reducer.

[0072] In this embodiment, it should be noted that the sodium lignin sulfonate water reducer was purchased from Shandong Qiansheng Chemical Co., Ltd.

[0073] In addition, this embodiment also provides a method for preparing the above-mentioned anti-splitting concrete containing modified polyester fibers, comprising the following steps:

[0074] Step 1: Accurately weigh silicate cement, quartz sand, aggregate, modified polyester fiber, hydrophobic agent, water reducing agent and water, and put silicate cement, quartz sand, aggregate and modified polyester fiber into a mixing device for mixing and stirring to obtain a mixture.

[0075] Among them, the rotation speed of the mixing equipment is 220r / min, and the mixing time is 25min.

[0076] Step 2: After the hydrophobic agent, water reducing agent and water are fully mixed, the mixture is added thereto, and the stirring and mixing is continued for 12 minutes. After the mixing is completed, the material is discharged, and finally a finished product of anti-splitting concrete containing modified polyester fiber is obtained.

[0077] Example 3

[0078] The preparation method of the modified polyester fiber-containing anti-split concrete provided in this embodiment is basically the same as that in Embodiment 1, except that: the specific raw material composition and the specific preparation method of the modified polyester fiber-containing anti-split concrete in this embodiment are different; the specific raw material composition and the specific preparation method of the modified polyester fiber-containing anti-split concrete in this embodiment are as follows:

[0079] A modified polyester fiber-containing anti-splitting concrete is composed of the following raw materials in parts by weight: 120 parts of Portland cement, 14 parts of quartz sand, 30 parts of aggregate, 8 parts of modified polyester fiber, 7 parts of hydrophobic agent, 10 parts of water reducing agent and 50 parts of water.

[0080] In this embodiment, it should be noted that the silicate cement is ordinary silicate cement P·O42.5, which is purchased from Hunan Xindingli New Material Technology Co., Ltd.

[0081] Among them, the aggregate is a mixture of modified clay and limestone in a mass ratio of 1:2.1.

[0082] Further, the preparation process of modified clay is as follows:

[0083] The clay was placed in a resistance furnace, heated to 700°C at a heating rate of 10°C / min, and kept at this temperature for 260 min;

[0084] Then the temperature was raised to 780°C at a heating rate of 6°C / min and kept at that temperature for 120min. After natural cooling, the mixture was placed in a pulverizing device and pulverized to 2.2mm to obtain a powder.

[0085] The nano-silicon dioxide was ultrasonically dispersed in deionized water at a dosage of 0.45 g / mL for 30 min to obtain a prepared solution;

[0086] The powder was placed in the prepared solution at a dosage ratio of 0.25 g / mL and treated at 140 r / min for 36 h. After filtration, it was dried at 80° C. to constant weight to obtain modified clay.

[0087] In this embodiment, it should be noted that limestone was purchased from Shenyang Elepox Chemical Co., Ltd., clay was purchased from Shijiazhuang Fengming Mineral Products Co., Ltd., and nano-silicon dioxide was purchased from Aladdin Reagent (Shanghai) Co., Ltd.

[0088] Among them, the preparation process of modified polyester fiber is as follows:

[0089] Taking polytetrafluoroethylene fiber, and subjecting it to electron beam irradiation to obtain pretreated polytetrafluoroethylene fiber;

[0090] The silane coupling agent KH560 was placed in an ethanol aqueous solution with a concentration of 84% at a mass ratio of 0.75:1, stirred at 240 r / min for 14 min, and then nano-silicon dioxide was added thereto, and stirring was continued for 80 min;

[0091] Then, the pretreated polytetrafluoroethylene fiber was added thereto, and ultrasonic treatment was performed for 50 minutes. After filtration, the fiber was washed with anhydrous ethanol and deionized water for 4 times respectively, and dried at 80° C. for 16 hours to obtain the modified polyester fiber.

[0092] Furthermore, the irradiation dose of the electron beam irradiation is 300 kGy, and the irradiation time is 12 s.

[0093] In addition, the added amount of nano-silicon dioxide is 1.4% by mass of the ethanol aqueous solution.

[0094] The addition amount of the pretreated polytetrafluoroethylene fiber is 6.3% of the mass of the ethanol aqueous solution.

[0095] Among them, the water reducer is polycarboxylic acid water reducer.

[0096] In this embodiment, it should be noted that the polycarboxylate water reducer was purchased from Wuhan Runxingyuan Technology Co., Ltd.

[0097] In addition, this embodiment also provides a method for preparing the above-mentioned anti-splitting concrete containing modified polyester fibers, comprising the following steps:

[0098] Step 1: Accurately weigh silicate cement, quartz sand, aggregate, modified polyester fiber, hydrophobic agent, water reducing agent and water, and put silicate cement, quartz sand, aggregate and modified polyester fiber into a mixing device for mixing and stirring to obtain a mixture.

[0099] Among them, the rotation speed of the mixing equipment is 320r / min, and the mixing time is 30min.

[0100] Step 2: After the hydrophobic agent, water reducing agent and water are fully mixed, the mixture is added thereto, and the stirring and mixing is continued for 15 minutes. After the mixing is completed, the material is discharged, and finally a finished product of anti-split concrete containing modified polyester fiber is obtained.

[0101] Comparative Example 1: The difference from Example 1 is that in this example, an equal amount of polytetrafluoroethylene fibers are used instead of modified polyester fibers.

[0102] Comparative Example 2: The difference from Example 1 is that the aggregate in this example is a mixture of modified clay and limestone in a mass ratio of 1:1.

[0103] Comparative Example 3: The difference from Example 1 is that the aggregate in this example is a mixture of modified clay and limestone in a mass ratio of 2:1.

[0104] Comparative Example 4: The difference from Example 1 is that the aggregate in this example is a mixture of clay and limestone in a mass ratio of 1:2.1.

[0105] Performance test: The concrete samples provided in Examples 1 to 3 and Comparative Examples 1 to 4 are marked as Examples 1 to 3 and Comparative Examples 1 to 4, respectively; and the relevant properties of the concrete provided in Examples 1 to 3 and Comparative Examples 1 to 4 are tested as follows:

[0106] 1. Mechanical test: The test method is GBT50081-2019 to test the 28d splitting tensile strength and 28d compressive strength.

[0107] 2. Water absorption test: The test method is to use Appendix F of DB32 / T3696-2019 "Concrete Water Absorption Test Method" to determine the water absorption of concrete.

[0108] The obtained test data are recorded in Table 1 and Table 2 below:

[0109] Table 1 Mechanical properties test results of each group of concrete

[0110] Group Compressive strength(MPa) Splitting tensile strength (MPa) Example 1 Group 76.4 4.45 Example 2 Group 76.2 4.43 Example 3 Group 75.9 4.41 Comparison group 1 55.4 2.98 Comparison of 2 groups 68.2 3.38 Comparison of 3 groups 67.8 3.43 Comparison of 4 groups 59.9 3.16

[0111] Table 2 Absorption performance test results of each group of concrete

[0112]

[0113]

[0114] By comparing and analyzing the relevant data in Table 1 and Table 2, it can be seen that the anti-split concrete containing modified polyester fibers prepared by the present invention not only has good mechanical properties, but also has excellent anti-seepage performance, effectively ensuring its quality. This shows that the anti-split concrete containing modified polyester fibers and the preparation method provided by the present invention have a broader market prospect and are more suitable for promotion.

[0115] In the present invention, silicate cement, quartz sand, aggregate, modified polyester fiber, hydrophobic agent, water reducing agent and water are used as raw materials. The silicate cement, quartz sand, aggregate and modified polyester fiber are put into a mixing device for mixing and stirring to obtain a mixture. The hydrophobic agent, water reducing agent and water are fully mixed, and then the mixture is added thereto, and the mixing is continued. After the mixing is completed, the material is discharged to finally obtain a finished product of anti-splitting concrete containing modified polyester fiber. The anti-splitting concrete containing modified polyester fiber prepared by the present invention not only has good mechanical properties, but also has excellent anti-seepage performance, and effectively guarantees its quality.

[0116] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0117] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A modified polyester fiber-containing anti-splitting concrete, characterized in that: The invention is composed of the following raw materials in parts by weight: 100-120 parts of silicate cement, 10-14 parts of quartz sand, 20-30 parts of aggregate, 5-8 parts of modified polyester fiber, 4-7 parts of hydrophobic agent, 6-10 parts of water reducing agent and 30-50 parts of water.

2. The anti-splitting concrete containing modified polyester fiber according to claim 1, characterized in that: The aggregate is prepared by mixing modified clay and limestone in a mass ratio of 1:1.8 to 2.

1.

3. The anti-splitting concrete containing modified polyester fiber according to claim 2, characterized in that: The preparation process of the modified clay is as follows: Place the clay in a resistance furnace, heat it to 650-700°C at a heating rate of 8-10°C / min, and keep it at this temperature for 240-260min; Then, the temperature is raised to 760-780°C at a heating rate of 4-6°C / min, and kept at this temperature for 100-120 minutes. After natural cooling, the mixture is placed in a pulverizing device and pulverized to 0.2-2.2 mm to obtain a powder. The nano-silicon dioxide is ultrasonically dispersed in deionized water at a dosage ratio of 0.12 to 0.45 g / mL for 20 to 30 minutes to obtain a prepared solution; The powder is placed in the prepared solution at a dosage ratio of 0.05-0.25 g / mL, and treated at 120-140 r / min for 30-36 hours. After filtration, it is dried at 70-80° C. to constant weight to obtain modified clay.

4. The anti-splitting concrete containing modified polyester fiber according to claim 1, characterized in that: The preparation process of the modified polyester fiber is as follows: Taking polytetrafluoroethylene fiber, and subjecting it to electron beam irradiation to obtain pretreated polytetrafluoroethylene fiber; The silane coupling agent KH560 is placed in an ethanol aqueous solution with a concentration of 80-84% at a mass ratio of 0.65-0.75:1, stirred at 120-240 r / min for 10-14 min, and then nano-silicon dioxide is added thereto, and stirring is continued for 70-80 min; Then, the pretreated polytetrafluoroethylene fiber is added thereto, and ultrasonic treatment is performed for 40 to 50 minutes. After filtration, the fiber is washed with anhydrous ethanol and deionized water for 2 to 4 times respectively, and dried at a temperature of 70 to 80° C. for 14 to 16 hours to obtain the modified polyester fiber.

5. The anti-splitting concrete containing modified polyester fiber according to claim 4, characterized in that: The irradiation dose of the electron beam irradiation is 200-300 kGy, and the irradiation time is 10-12 s.

6. The anti-splitting concrete containing modified polyester fiber according to claim 4, characterized in that: The added amount of the nano silicon dioxide is 1.2-1.4% of the mass of the ethanol aqueous solution.

7. The anti-splitting concrete containing modified polyester fiber according to claim 4, characterized in that: The addition amount of the pretreated polytetrafluoroethylene fiber is 4.3-6.3% of the mass of the ethanol aqueous solution.

8. The anti-splitting concrete containing modified polyester fiber according to claim 1, characterized in that: The water reducer is selected from any one of polycarboxylic acid water reducer and sodium lignin sulfonate water reducer.

9. A method for preparing split-resistant concrete containing modified polyester fiber according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1, accurately weighing silicate cement, quartz sand, aggregate, modified polyester fiber, hydrophobic agent, water reducing agent and water, and putting silicate cement, quartz sand, aggregate and modified polyester fiber into a mixing device for mixing and stirring to obtain a mixture; Step 2: After the hydrophobic agent, water reducing agent and water are fully mixed, the mixture is added thereto, and the stirring and mixing is continued for 10 to 15 minutes. After the mixing is completed, the material is discharged to finally obtain a finished product of anti-splitting concrete containing modified polyester fiber.

10. The method for preparing split-resistant concrete containing modified polyester fiber according to claim 1, characterized in that: In the step 1, the rotation speed of the mixing equipment is 120 to 320 r / min, and the mixing time is 20 to 30 min.

Citation Information

Patent Citations

  • C35 basalt fiber concrete for bridge abutment and preparation method of C35 basalt fiber concrete

    CN112159168A

  • Low-carbon low-shrinkage engineering cement-based composite material and preparation method thereof

    CN116903334A