Preparation method of oxidation sensor with built-in large cavity
By using a combination of PVB particles with a particle size of 1–3 μm and volatile organic solvents in the oxidation sensor to form a micro-film structure, the problems of insufficient cavity volume and high cracking rate are solved, achieving high yield and high precision oxygen detection.
Patent Information
- Application Number
- CN202410989695.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing limiting current type oxygen sensor cannot increase the cavity volume, and the finished product is prone to cracking when the amount of adhesive applied is large.
A two-stage adhesive is prepared by uniformly dispersing PVB particles with a particle size of 1-3 μm in a volatile organic solvent. The adhesive is then laminated by isostatic pressing with warm water to form a micro-film structure. The amount of adhesive applied is controlled to ensure the adhesion of the green ceramic tiles and prevent cracking.
With a cavity ratio of over 30%, the cracking rate of the oxidation sensor is less than 2%, resulting in a high yield and more accurate and faster detection of oxygen content.
Smart Images

Figure BDA0004958514280000081 
Figure BDA0004958514280000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oxidation sensors, and in particular to a preparation method of a built-in large-cavity oxidation sensor. Background Art
[0002] The chip oxygen sensor is a relatively new oxygen sensor. It has the advantages of short response time, small size, low manufacturing cost, and reliable performance. It is an important component for the automotive industry to achieve energy conservation and emission reduction, improve fuel economy, and reduce harmful gas emissions from automobile exhaust. The oxygen sensor chip is the core of the chip oxygen sensor and also the main component. The oxygen sensor can measure the oxygen content in the engine exhaust and determine whether the gasoline and air are completely burned. The electronic controller implements closed-loop control with the excess air coefficient λ=1 as the target based on the feedback information of the oxygen sensor to ensure that the three-way catalytic converter has the maximum conversion efficiency for the three pollutants of HC, CO and NOx in the exhaust.
[0003] At present, the limiting current type chip oxygen sensor with cavity has attracted much attention. It can work under steady-state oxygen flow and can more easily test the content of oxygen and nitric oxide. For example, a dual-cell current type nitrogen oxide sensor chip and preparation method disclosed in publication number CN105973965B, which consists of a three-layer tablet, an electrode is formed on the substrate by screen printing, and then the substrate is formed into an oxygen sensor by stacking and sintering. The structure is simple and the preparation method is easier to operate; the cavity of the limiting current type chip oxygen sensor provides oxygen to the reverse electrode, so the oxygen flow rate of the large cavity will increase, thereby increasing the reverse current value, making it easier to measure oxygen. The gas content is identified and processed; however, the current cavity is formed by printing carbon, but the cavity formed by brushing carbon can only reach 30% of the cavity rate. In addition, a groove can be formed on the substrate by punching, and then a cavity is formed by gluing, stacking and sintering. However, when punching first and then gluing, it is difficult to control the amount of glue due to the large proportion of the cavity, and in order to enable the stacking to be effectively stacked, the amount of glue applied to the stacking is usually large, so a thicker glue film will be formed between the stacking sheets, and this part of the glue film will prevent the stacking sheets from being effectively bonded and formed into a whole during the subsequent sintering, resulting in the rear oxygen sensor being easy to crack after forming. Summary of the invention
[0004] The present invention aims at the problem that the cavity volume of the limiting current type oxygen sensor in the prior art cannot be increased and the finished product is prone to cracking due to a large amount of glue applied. The present invention provides a preparation method for an oxidation sensor with a built-in large cavity. The oxidation sensor prepared by the method has a cracking rate of less than 2% under the condition of a cavity ratio of more than 30%, a high yield and a simple process, and optimizes the glue material and the lamination pressing method. The glue material of the present invention selects PVB glue particles with a particle size of 1 to 3 μm and evenly disperses them in a volatile organic solvent to prepare a two-stage glue material. By controlling the particle size ratio of the PVB glue particles, the effect of precise glue application can be achieved, and the glue particles can be evenly sprayed on the composite surface of a raw ceramic sheet with a smaller area. These glue particles will form a tiny membrane structure between the raw ceramic sheets after being laminated by warm water isostatic pressing to provide adhesion to the raw ceramic sheets, thereby ensuring that the blocks composed of the raw ceramic sheets will not collapse in structure. At the same time, when the blocks are sintered, the volume change of the ceramic sheets due to thermal expansion will fill the membrane structure so that the raw ceramic sheets are in contact and sintered into a whole, which can significantly reduce the cracking rate of the oxidation sensor.
[0005] The specific technical scheme of the present invention is: A method for preparing a built-in large cavity oxidation sensor comprises the following steps: The green porcelain pieces are pre-treated to form green porcelain fragments, the pre-treatment includes a first stage of glue spraying and a first stage of warm water isostatic pressing, the green porcelain fragments are overlapped to form green embryo blocks, the overlapped treatment includes two stages of glue spraying and two stages of warm water isostatic pressing, and the green embryo blocks are sintered to form a built-in large cavity oxidation sensor; The conditions of the two-stage glue spraying treatment include: spraying the second-stage glue, the second-stage glue is PVB and volatile organic solvent, the PVB content is 10-30%, the particle size of the PVB is 1-3 μm, and the spraying density of the PVB is 50 to 70; The conditions of the second stage warm water isostatic pressing treatment include: temperature 60-80° C., pressure 5-20 MPa, and pressure holding time 5-60 min.
[0006] The present invention provides a method for preparing an oxidation sensor with a built-in large cavity. The oxidation sensor prepared by the method has a finished product cracking rate of less than 2% under the condition of a cavity ratio of 30%, a high yield rate and a simple process. The larger the cavity of the current-type oxidation sensor, the greater the oxygen flow rate in the cavity, and the greater the reverse current value, so that the sensor can detect the oxygen content in the gas more accurately and quickly. The cavity ratio of the oxidation sensor prepared by the existing technology using the carbon brushing method can only reach 30% at most. In addition, although the method of directly using punching to make the cavity can obtain a higher cavity ratio, the oxidation sensor prepared by punching and then compounding is The cracking rate is extremely high, and the greater the proportion of the cavity, the higher the cracking rate of the oxidation sensor. The reason for the above problem is that the cavity ratio of the raw porcelain sheet becomes larger after punching, which reduces the area where the raw porcelain sheets can be stacked. In the prior art, when stacking the raw porcelain sheets, it is necessary to first bond the raw porcelain sheets with glue, and then sinter the raw porcelain sheets into a whole through high-temperature sintering. However, the glue in the prior art has a high viscosity when used, and will form a thicker film structure between the raw porcelain sheets. This partial film structure will make it impossible for adjacent raw porcelain sheets to be in contact during sintering, resulting in cracks, which makes the manufactured oxidation sensor prone to cracking.
[0007] In view of the above problems, the present invention optimizes the glue and the lamination pressing method. The present invention selects PVB glue particles with a particle size of 1 to 3 μm and evenly disperses them in a volatile organic solvent to form a two-stage glue. By controlling the particle size and proportion of the PVB glue particles, the effect of precise sizing can be achieved, and the glue particles can be evenly sprayed on the composite surface of the raw ceramic sheet with a smaller area. After these glue particles are laminated by warm water isostatic pressing, a tiny film structure will be formed between the raw ceramic sheets to provide adhesion to the raw ceramic sheets, ensuring that the blocks composed of the raw ceramic sheets will not collapse in structure. At the same time, when the tiny membrane structure is sintered in the block, the volume change of the ceramic sheet due to thermal expansion will fill the membrane structure so that the raw ceramic sheets are in contact and sintered into a whole, which can significantly reduce the cracking rate of the oxidation sensor. The present invention uses a volatile organic solvent to evenly disperse the PVB particles, so that the smaller PVB particles will not agglomerate, and the PVB particles exist in the form of single particles on the surface of the raw ceramic sheet. In addition, the volatile solvent evaporates after spraying, leaving only the PVB particles, without residue, and will not affect the subsequent steps.
[0008] The present invention does not limit the first stage of adhesive when preparing raw porcelain fragments. The reason is that the first stage of warm water isostatic pressing treatment adopts a high pressure treatment. When preparing raw porcelain fragments, it is necessary to use a high pressure treatment to make the raw porcelain pieces directly solidify into a sensor functional area with an integrated structure. Therefore, the first stage of adhesive is only for fixing the raw porcelain pieces. After applying the first stage of adhesive, it can be directly loaded into the warm water isostatic pressing treatment device for a warm water isostatic pressing treatment. When the raw porcelain fragments are made into blocks, a large pressure cannot be used. The functional area of the sensor needs to be sintered into a whole by sintering. Therefore, the second stage of adhesive needs to accurately control the amount of adhesive applied to ensure that the PVB glue particles form a tiny membrane structure between the raw porcelain pieces and provide bonding force.
[0009] Preferably, the conditions of the warm water isostatic pressing treatment include: temperature 60-80° C., time 5-100 s, and pressure 5-30 t.
[0010] Preferably, the conditions for the one-stage glue spraying treatment include: spraying a stage of glue, wherein the stage of glue is PVB and a volatile organic solvent, and the content of PVB is 10-30%.
[0011] Preferably, the volatile organic solvent is anhydrous ethanol.
[0012] Preferably, the pre-treatment also includes a punching process and an inner electrode printing process.
[0013] Preferably, the punching process is one or both of mechanical punching and laser punching; and the slurry used in the inner electrode printing process is platinum slurry.
[0014] Preferably, the green ceramic sheet is one or both of an alumina green ceramic sheet and a zirconia green ceramic sheet.
[0015] Preferably, the content of alumina in the alumina green ceramic sheet is greater than 99 wt%.
[0016] Preferably, the content of zirconium oxide in the zirconium oxide green ceramic sheet is greater than 99 wt %.
[0017] Preferably, the sintering conditions are: sintering temperature 1500-2000° C., and sintering time 2-3 hours.
[0018] Compared with the prior art, this application has the following technical effects: The present invention provides a preparation method of an oxidation sensor with a built-in large cavity, wherein the method optimizes the adhesive and the lamination pressing mode. The adhesive of the present invention selects PVB particles with a particle size of 1 to 3 μm and evenly disperses them in a volatile organic solvent to form a two-stage adhesive. The particle size and content of the PVB particles can be controlled to achieve the effect of precise sizing, and the particles can be evenly sprayed on the composite surface of a raw ceramic sheet with a smaller area. These particles are then laminated by warm water isostatic pressing to form a tiny membrane structure between the raw ceramic sheets to provide adhesion to the raw ceramic sheets. When the tiny membrane structure is sintered, the volume change of the ceramic sheet due to thermal expansion will fill the membrane structure so that the raw ceramic sheets are in contact and sintered into a whole, thereby ensuring that the structure of the raw embryo block will not collapse and significantly reducing the cracking rate of the oxidation sensor. DETAILED DESCRIPTION
[0019] The present invention will be further described below in conjunction with the embodiments.
[0020] Embodiment 1: A method for preparing a built-in large cavity oxidation sensor comprises the following steps: Preparation of green porcelain fragments: 11 alumina green porcelain sheets with a thickness of 185 μm and 1 zirconia green porcelain sheet with a thickness of 185 μm are numbered and placed at 60°C for drying for 15 minutes for use, and No. 1 to 4 alumina green porcelain sheets are used as heater areas, No. 5 to 8 alumina green porcelain sheets are used as large cavity areas, and No. 9 zirconia green porcelain sheets and No. 10 to 12 alumina green porcelain sheets are used as electrode areas; internal electrodes are printed on the green porcelain sheets in the heater area according to pattern requirements, and internal electrodes are printed on the green porcelain sheets in the electrode area of the heater area according to pattern requirements, and the printing slurry is platinum slurry; a stage of sizing is used to apply sizing to the green porcelain sheets, and the stage of sizing is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 10%, and the polymerization degree of PVB is 5000). After applying the sizing, the green porcelain sheets are stacked according to the numbers and subjected to a stage of warm water, etc. The green porcelain fragments of the heater area, the green porcelain fragments of the large cavity area and the green porcelain fragments of the electrode area are respectively made by static pressing; the conditions of the first stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 40MPa for 20 minutes; preparing green embryo blocks: using a second stage of glue to apply glue to the green porcelain fragments, the first stage of glue is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 10%, the polymerization degree of PVB is 5000, and the particle size of PVB is 1-3μm), after applying glue, the green porcelain fragments of the heater, the green porcelain fragments of the large cavity and the green porcelain fragments of the electrode area are sequentially overlapped, and after overlapping, two stages of warm water isostatic pressing are performed to form green embryo blocks; the conditions of the second stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 15MPa for 40 minutes; Preparation of built-in large cavity oxidation sensor: After heating the green embryo block at 60℃ for 10 minutes, use special cutting equipment to cut it into a single built-in large cavity oxygen sensor green embryo unit, place the built-in large cavity oxygen sensor green embryo unit on a supporting plate, place it in a sintering device, sinter it at 1500℃ for 2 hours, and then cool it to make a built-in large cavity oxidation sensor.
[0021] Embodiment 2: A method for preparing a built-in large cavity oxidation sensor comprises the following steps: Preparation of green porcelain fragments: 12 alumina green porcelain sheets with a thickness of 185 μm and 1 zirconia green porcelain sheet with a thickness of 185 μm are numbered and placed at 60°C for drying for 15 minutes for use, and No. 1 to 4 alumina green porcelain sheets are used as heater areas, No. 5 to 9 alumina green porcelain sheets are used as large cavity areas, and No. 10 zirconia green porcelain sheets and No. 11 to 13 alumina green porcelain sheets are used as electrode areas; internal electrodes are printed on the green porcelain sheets in the heater area according to pattern requirements, and internal electrodes are printed on the green porcelain sheets in the electrode area of the heater area according to pattern requirements, and the printing slurry is platinum slurry; a stage of sizing is used to apply sizing to the green porcelain sheets, and the stage of sizing is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 20%, and the polymerization degree of PVB is 5000). After applying the sizing, the green porcelain sheets are stacked according to the numbers and subjected to a stage of warm water, etc. The green porcelain fragments of the heater area, the green porcelain fragments of the large cavity area and the green porcelain fragments of the electrode area are respectively made by static pressing; the conditions of the first stage of warm water isostatic pressing are: preheating at 70°C for 10 minutes and maintaining the pressure at a pressure of 40MPa for 20 minutes; preparing green embryo blocks: using a second stage of glue to apply glue to the green porcelain fragments, the first stage of glue is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 20%, the polymerization degree of PVB is 5000, and the particle size of PVB is 1-3μm), after applying glue, the green porcelain fragments of the heater, the green porcelain fragments of the large cavity and the green porcelain fragments of the electrode area are sequentially overlapped, and after overlapping, two stages of warm water isostatic pressing are performed to form green embryo blocks; the conditions of the second stage of warm water isostatic pressing are: preheating at 60°C for 10 minutes and maintaining the pressure at a pressure of 14MPa for 40 minutes; Preparation of built-in large cavity oxidation sensor: After heating the green embryo block at 60℃ for 10 minutes, use special cutting equipment to cut it into a single built-in large cavity oxygen sensor green embryo unit, place the built-in large cavity oxygen sensor green embryo unit on a supporting plate, place it in a sintering device, sinter it at 1500℃ for 2 hours, and then cool it to make a built-in large cavity oxidation sensor.
[0022] Embodiment 3: A method for preparing a built-in large cavity oxidation sensor comprises the following steps: Preparation of green porcelain fragments: 13 alumina green porcelain sheets with a thickness of 185 μm and 1 zirconia green porcelain sheet with a thickness of 185 μm are numbered and placed at 60°C for drying for 15 minutes for use, and the alumina green porcelain sheets No. 1 to 4 are used as the heater area, the alumina green porcelain sheets No. 5 to 10 are used as the large cavity area, and the zirconia green porcelain sheets No. 11 and the alumina green porcelain sheets No. 12 to 14 are used as the electrode area; the inner electrode is printed on the green porcelain sheets in the heater area according to the pattern requirements, and the inner electrode is printed on the green porcelain sheets in the electrode area of the heater area according to the pattern requirements, and the printing slurry is platinum slurry; a stage of sizing is used to apply sizing to the green porcelain sheets, and the stage of sizing is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 30%, and the polymerization degree of PVB is 5000). After applying the sizing, the green porcelain sheets are stacked according to the numbers and subjected to a stage of warm water The green porcelain fragments of the heater area, the green porcelain fragments of the large cavity area and the green porcelain fragments of the electrode area are respectively prepared by isostatic pressing; the conditions of the first stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 40MPa for 20 minutes; preparing green embryo blocks: using a second stage of glue to apply glue to the green porcelain fragments, the first stage of glue is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 30%, the polymerization degree of PVB is 5000, and the particle size of PVB is 1-3μm), after applying glue, the green porcelain fragments of the heater, the green porcelain fragments of the large cavity and the green porcelain fragments of the electrode area are sequentially overlapped, and after overlapping, two stages of warm water isostatic pressing are performed to prepare green embryo blocks; the conditions of the second stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 13MPa for 40 minutes; Preparation of built-in large cavity oxidation sensor: After heating the green embryo block at 60℃ for 10 minutes, use special cutting equipment to cut it into a single built-in large cavity oxygen sensor green embryo unit, place the built-in large cavity oxygen sensor green embryo unit on a supporting plate, place it in a sintering device, sinter it at 1500℃ for 2 hours, and then cool it to make a built-in large cavity oxidation sensor.
[0023] Embodiment 4: A method for preparing a built-in large cavity oxidation sensor comprises the following steps: Preparation of green porcelain fragments: 12 alumina green porcelain sheets with a thickness of 185 μm and 1 zirconia green porcelain sheet with a thickness of 185 μm are numbered and placed at 60°C for drying for 15 minutes for use, and No. 1 to 4 alumina green porcelain sheets are used as heater areas, No. 5 to 9 alumina green porcelain sheets are used as large cavity areas, and No. 10 zirconia green porcelain sheets and No. 11 to 13 alumina green porcelain sheets are used as electrode areas; internal electrodes are printed on the green porcelain sheets in the heater area according to pattern requirements, and internal electrodes are printed on the green porcelain sheets in the electrode area of the heater area according to pattern requirements, and the printing slurry is platinum slurry; a section of glue is used to apply glue to the green porcelain sheets, and the section of glue is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 30%, and the polymerization degree of PVB is 5000). After applying glue, the green porcelain sheets are stacked according to the numbers and subjected to a section of warm water, etc. The green porcelain fragments of the heater area, the green porcelain fragments of the large cavity area and the green porcelain fragments of the electrode area are respectively made by static pressing; the conditions of the first stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 40MPa for 20 minutes; preparing green embryo blocks: using a second stage of glue to apply glue to the green porcelain fragments, the first stage of glue is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 30%, the polymerization degree of PVB is 5000, and the particle size of PVB is 1-3μm), after applying glue, the green porcelain fragments of the heater, the green porcelain fragments of the large cavity and the green porcelain fragments of the electrode area are sequentially overlapped, and after overlapping, two stages of warm water isostatic pressing are performed to form green embryo blocks; the conditions of the second stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 14MPa for 40 minutes; Preparation of built-in large cavity oxidation sensor: After heating the green embryo block at 60℃ for 10 minutes, use special cutting equipment to cut it into a single built-in large cavity oxygen sensor green embryo unit, place the built-in large cavity oxygen sensor green embryo unit on a supporting plate, place it in a sintering device, sinter it at 1500℃ for 2 hours, and then cool it to make a built-in large cavity oxidation sensor.
[0024] Embodiment 5: A method for preparing a built-in large cavity oxidation sensor comprises the following steps: Preparation of green porcelain fragments: 13 alumina green porcelain sheets with a thickness of 185 μm and 1 zirconia green porcelain sheet with a thickness of 185 μm are numbered and placed at 60°C for drying for 15 minutes for use, and No. 1 to 4 alumina green porcelain sheets are used as heater areas, No. 5 to 10 alumina green porcelain sheets are used as large cavity areas, and No. 11 zirconia green porcelain sheets and No. 12 to 14 alumina green porcelain sheets are used as electrode areas; internal electrodes are printed on the green porcelain sheets in the heater area according to pattern requirements, and internal electrodes are printed on the green porcelain sheets in the electrode area of the heater area according to pattern requirements, and the printing slurry is platinum slurry; a stage of sizing is used to apply sizing to the green porcelain sheets, and the stage of sizing is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 20%, and the polymerization degree of PVB is 5000). After applying the sizing, the green porcelain sheets are stacked according to the numbers and subjected to a stage of warm water slurry. The green porcelain fragments of the heater area, the green porcelain fragments of the large cavity area and the green porcelain fragments of the electrode area are respectively made by isostatic pressing; the conditions of the first stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 40MPa for 20 minutes; preparing green embryo blocks: using a second stage of glue to apply glue to the green porcelain fragments, the first stage of glue is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 20%, the polymerization degree of PVB is 5000, and the particle size of PVB is 1-3μm), after applying glue, the green porcelain fragments of the heater, the green porcelain fragments of the large cavity and the green porcelain fragments of the electrode area are sequentially superimposed, and after superposition, two stages of warm water isostatic pressing are performed to form green embryo blocks; the conditions of the second stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 13MPa for 40 minutes; Preparation of built-in large cavity oxidation sensor: After heating the green embryo block at 60℃ for 10 minutes, use special cutting equipment to cut it into a single built-in large cavity oxygen sensor green embryo unit, place the built-in large cavity oxygen sensor green embryo unit on a supporting plate, place it in a sintering device, sinter it at 1500℃ for 2 hours, and then cool it to make a built-in large cavity oxidation sensor.
[0025] Embodiment 6: A method for preparing a built-in large cavity oxidation sensor comprises the following steps: Preparation of green porcelain fragments: 13 alumina green porcelain sheets with a thickness of 185 μm and 1 zirconia green porcelain sheet with a thickness of 185 μm are numbered and placed at 60°C for drying for 15 minutes for use, and No. 1 to 4 alumina green porcelain sheets are used as heater areas, No. 5 to 10 alumina green porcelain sheets are used as large cavity areas, and No. 11 zirconia green porcelain sheets and No. 12 to 14 alumina green porcelain sheets are used as electrode areas; internal electrodes are printed on the green porcelain sheets in the heater area according to pattern requirements, and internal electrodes are printed on the green porcelain sheets in the electrode area of the heater area according to pattern requirements, and the printing slurry is platinum slurry; a stage of sizing is used to apply sizing to the green porcelain sheets, and the stage of sizing is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 20%, and the polymerization degree of PVB is 5000). After applying the sizing, the green porcelain sheets are stacked according to the numbers and subjected to a stage of warm water slurry. The green porcelain fragments of the heater area, the green porcelain fragments of the large cavity area and the green porcelain fragments of the electrode area are respectively prepared by isostatic pressing; the conditions of the first stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 40MPa for 20 minutes; preparing green embryo blocks: using a second stage of glue to apply glue to the green porcelain fragments, the first stage of glue is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 20%, the polymerization degree of PVB is 5000, and the particle size of PVB is 1-3μm), after applying glue, the green porcelain fragments of the heater, the green porcelain fragments of the large cavity and the green porcelain fragments of the electrode area are sequentially overlapped, and after overlapping, two stages of warm water isostatic pressing are performed to prepare green embryo blocks; the conditions of the second stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 10MPa for 40 minutes; Preparation of built-in large cavity oxidation sensor: After heating the green embryo block at 60℃ for 10 minutes, use special cutting equipment to cut it into a single built-in large cavity oxygen sensor green embryo unit, place the built-in large cavity oxygen sensor green embryo unit on a supporting plate, place it in a sintering device, sinter it at 1500℃ for 2 hours, and then cool it to make a built-in large cavity oxidation sensor.
[0026] Embodiment 7: A method for preparing a built-in large cavity oxidation sensor comprises the following steps: Preparation of green porcelain fragments: 13 alumina green porcelain sheets with a thickness of 185 μm and 1 zirconia green porcelain sheet with a thickness of 185 μm are numbered and placed at 60°C for drying for 15 minutes for use, and No. 1 to 4 alumina green porcelain sheets are used as heater areas, No. 5 to 10 alumina green porcelain sheets are used as large cavity areas, and No. 11 zirconia green porcelain sheets and No. 12 to 14 alumina green porcelain sheets are used as electrode areas; internal electrodes are printed on the green porcelain sheets in the heater area according to pattern requirements, and internal electrodes are printed on the green porcelain sheets in the electrode area of the heater area according to pattern requirements, and the printing slurry is platinum slurry; a stage of sizing is used to apply sizing to the green porcelain sheets, and the stage of sizing is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 20%, and the polymerization degree of PVB is 5000). After applying the sizing, the green porcelain sheets are stacked according to the numbers and subjected to a stage of warm water slurry. The green porcelain fragments of the heater area, the green porcelain fragments of the large cavity area and the green porcelain fragments of the electrode area are respectively prepared by isostatic pressing; the conditions of the first stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 40MPa for 20 minutes; preparing green embryo blocks: using a second stage of glue to apply glue to the green porcelain fragments, the first stage of glue is a dispersed mixture of PVB and anhydrous ethanol (the PVB content is 20%, the polymerization degree of PVB is 5000, and the particle size of PVB is 1-3μm), after applying glue, the green porcelain fragments of the heater, the green porcelain fragments of the large cavity and the green porcelain fragments of the electrode area are sequentially overlapped, and after overlapping, two stages of warm water isostatic pressing are performed to prepare green embryo blocks; the conditions of the second stage of warm water isostatic pressing are: preheating at 80°C for 10 minutes and maintaining the pressure at a pressure of 11MPa for 40 minutes; Preparation of built-in large cavity oxidation sensor: After heating the green embryo block at 60℃ for 10 minutes, use special cutting equipment to cut it into a single built-in large cavity oxygen sensor green embryo unit, place the built-in large cavity oxygen sensor green embryo unit on a supporting plate, place it in a sintering device, sinter it at 1500℃ for 2 hours, and then cool it to make a built-in large cavity oxidation sensor.
[0027] Comparative Example 1: Compared with Example 1, the first-stage rubber compound and the second-stage rubber compound of Comparative Example 1 were not dispersed using anhydrous ethanol, and the other conditions were the same as those of Example 1.
[0028] Comparative Example 2: Compared with Example 1, the second-stage rubber material and the first-stage rubber material in Comparative Example 2 (the PVB content is 20%, and the polymerization degree of PVB is 10000), and the other conditions are the same as those in Example 1.
[0029] Comparative Example 3: Compared with Example 1, the second stage warm water isostatic pressing of Comparative Example 3 is maintained at a pressure of 20 MPa for 40 minutes, and the other conditions are the same as those of Example 1.
[0030] Comparative Example 4: Compared with Example 1, Comparative Example 4 adopts a carbon brushing process to prepare an oxidation sensor.
[0031] Test example 1: The oxidation sensors prepared in Examples 1 to 7 and Comparative Examples 1 to 5 were tested, and the test items included: cavity ratio, reverse current, and cracking rate; The cavity ratio test uses X-ray equipment to measure the cavity area; The reverse current test method is: provide 12V voltage to the heater, provide 0.45V voltage to the electrode, connect the reverse electrode to measure and read the current; The cracking rate test method is: after absorbing blue, full inspection at CCD15 magnification; The test results are shown in Table 1; Table 1 Test results As shown in Table 1, in Examples 1 to 7, the cracking rate is between 0.3% and 1.8% when the cavity ratio is 30-38%. Under the condition of large cavity, the cracking rate can be significantly reduced to below 2%, which significantly improves the yield of the oxidation sensor.
[0032] In Comparative Example 1, anhydrous ethanol was not used for dispersion. The cracking rate of Comparative Example 1 reached 51.5% under the condition of 30% cavity ratio. The cracking rate of Comparative Example 1 was significantly improved compared with Example 1. After analysis, it was found that the PVB glue powder that was not dispersed with anhydrous ethanol could not be evenly dispersed on the surface of the raw porcelain sheet composite surface. At the same time, the PVB glue particles would agglomerate and could not exist in the form of single particles on the surface of the raw porcelain sheet. Therefore, a thicker film structure would be formed at the composite of the raw porcelain sheet after composite, resulting in a significantly increased cracking rate of the oxidation sensor finally formed.
[0033] In Comparative Example 2, the second-stage rubber material is the same as the first-stage rubber material, and the particle size and proportion of the second-stage rubber material are not limited. The cracking rate of Comparative Example 2 reaches 33.1% under the condition of 30% cavity proportion, and the cracking rate of Comparative Example 2 is significantly improved compared with Example 1. The first-stage rubber material used in the example is PVB with a polymerization degree of 20,000, and the particle size of the PVB particles is 20-40 μm. The results of Comparative Example 2 and Example 1 show that when the PVB particles are too large, the film structure formed between the composite surfaces of the raw porcelain sheets will increase significantly, so that the cracking rate of the oxidation sensor finally formed is significantly increased.
[0034] In Comparative Example 3, the second stage warm water isostatic pressing was set to a high pressure. It was found that the cracking rate of the oxidation sensor in Comparative Example 3 reached 76.8%. The above results show that the second stage warm water isostatic pressing cannot be performed at a high pressure, and a high pressure will cause a significant increase in the cracking rate of the oxidation sensor.
[0035] Comparative Example 4 adopts the carbon brushing process in the prior art. The results of Comparative Example 4 show that when the cavity proportion reaches 18%, the cracking rate of the carbon brushing process reaches 5%, and when the cavity proportion is 30%, the cracking rate increases to 80%. The method provided in the present application has a significant advantage in that the cracking rate of the oxidation sensor is less than 2% under the condition of a cavity proportion of 30%.
[0036] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a built-in large cavity oxidation sensor, characterized in that: The following steps are involved: The green porcelain pieces are pre-treated to form green porcelain fragments, the pre-treatment includes a first stage of glue spraying and a first stage of warm water isostatic pressing, the green porcelain fragments are overlapped to form green embryo blocks, the overlapped treatment includes two stages of glue spraying and two stages of warm water isostatic pressing, and the green embryo blocks are sintered to form a built-in large cavity oxidation sensor; The conditions of the two-stage glue spraying treatment include: spraying the second-stage glue, the second-stage glue is PVB and volatile organic solvent, the PVB content is 10-30%, the particle size of the PVB is 1-3 μm, and the spraying density of the PVB is 50 to 70; The conditions of the second stage warm water isostatic pressing treatment include: temperature 60-80°C, pressure 5-20 MPa, and pressure holding time 5-60 min.
2. The method for preparing a built-in large cavity oxidation sensor according to claim 1, characterized in that: The conditions of the one-stage warm water isostatic pressing treatment include: temperature 60-80°C, time 5-100 s, and pressure 30-50 Mpa.
3. The method for preparing a built-in large cavity oxidation sensor according to claim 1, characterized in that: The conditions of the one-stage glue spraying treatment include: spraying a stage of glue, wherein the stage of glue is PVB and a volatile organic solvent, and the content of PVB is 10-30%.
4. The method for preparing a built-in large cavity oxidation sensor according to claim 1 or 3, characterized in that: The volatile organic solvent is anhydrous ethanol.
5. The method for preparing a built-in large cavity oxidation sensor according to claim 1, characterized in that: The pre-processing also includes punching processing and inner electrode printing processing.
6. The method for preparing a built-in large cavity oxidation sensor according to claim 5, characterized in that: The punching process is one or both of mechanical punching and laser punching; the slurry used in the inner electrode printing process is platinum slurry.
7. The method for preparing a built-in large cavity oxidation sensor according to claim 1, characterized in that: The green ceramic sheets are one or both of aluminum oxide green ceramic sheets and zirconium oxide green ceramic sheets.
8. The method for preparing a built-in large cavity oxidation sensor according to claim 7, characterized in that: The content of aluminum oxide in the aluminum oxide green ceramic sheet is greater than 99 wt %.
9. The method for preparing a built-in large cavity oxidation sensor according to claim 7, characterized in that: The content of zirconium oxide in the zirconium oxide green ceramic sheet is greater than 99 wt %.
10. The method for preparing a built-in large cavity oxidation sensor according to claim 1, characterized in that: The sintering conditions are: sintering temperature 1500-2000° C., and sintering time 2-3 hours.