Piezoelectric ceramic material, preparation method thereof and piezoelectric device
By modifying and doping Ca0.05Bi2.97Ti1-y(Ni1/6Zn1/6Ta2/3)yNbO9 on bismuth calcium titanate ceramics, (1-x)CaBi4Ti4O15·xCa0.05Bi2.97Ti1-y(Ni1/6Zn1/ 6Ta2/3)yNbO9 piezoelectric ceramic material solves the problem of insufficient piezoelectric constant and resistivity in high temperature environments, and achieves higher piezoelectric properties and resistivity.
Patent Information
- Application Number
- CN202411091671.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing bismuth calcium titanate ceramics have insufficient piezoelectric constant and high-temperature resistivity in high-temperature environments, which cannot meet the requirements of high-end piezoelectric devices.
By modifying and doping Ca0.05Bi2.97Ti1-y(Ni1/6Zn1/6Ta2/3)yNbO9 on bismuth calcium titanate ceramics, the chemical general formula is (1-x)CaBi4Ti4O15·xCa0.05Bi2.97Ti1-y( Ni1/6Zn1/6Ta2/3) yNbO9 piezoelectric ceramic material uses solid phase sintering and prefiring steps to increase its piezoelectric constant and high-temperature resistivity.
While maintaining a high Curie temperature, the piezoelectric constant and high-temperature resistivity of piezoelectric ceramic materials are significantly improved, making it suitable for high-temperature conditions, with a piezoelectric constant not less than 12pC/N, and a high-temperature resistivity of 600℃ is not low. at 8.1×105Ω·cm.
Smart Images

Figure CN118930254A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of piezoelectric ceramics, and in particular to a piezoelectric ceramic material, a preparation method thereof, and a piezoelectric device. Background Art
[0002] Materials with piezoelectric properties are called piezoelectric materials. As a material that can realize the mutual coupling function of mechanical energy and electrical energy, it is widely used in the industrial field, especially in aerospace, geological exploration and other fields. Piezoelectric materials can generally be divided into four categories: piezoelectric ceramics, piezoelectric single crystals, piezoelectric polymers and piezoelectric composite materials. Among them, piezoelectric ceramics have many advantages such as simple process, strong repeatability, low cost, adjustable components, and excellent performance, so they are favored by the market.
[0003] At present, the most mature and widely used piezoelectric ceramics are mainly PZT-based ceramics, but due to the high-temperature depolarization of piezoelectric properties, the use temperature of this type of ceramics generally does not exceed 300°C. However, in actual application environments, piezoelectric devices need to serve at temperatures of 600°C or even higher. Therefore, it is very necessary to study piezoelectric materials with excellent piezoelectric properties and high use temperatures.
[0004] Lead-free bismuth layered ceramics have the advantages of high Curie temperature, good temperature stability, and environmental friendliness, and are a candidate material suitable for use in high-temperature environments. Bismuth layered ceramics are made of (Bi2O2) 2+ The chemical formula of the perovskite-like layer is (Bi2O2). 2+ (A m-1 B m O 3m+1 ) 2- , of which calcium bismuth titanate CaBi4Ti4O 15 Ceramics have the advantages of ideal high Curie point (Tc = 790 ° C) and high depolarization temperature, but the piezoelectric constant (d 33 ) and 600℃ high temperature resistivity is low, that is, d 33 Only 8pC / N, 600℃ high temperature resistivity 1.1×10 5 Ω·cm, which cannot meet the requirements of high-end piezoelectric devices. Summary of the invention
[0005] Based on the above-mentioned deficiencies, the present application provides a piezoelectric ceramic material, a preparation method thereof and a piezoelectric device to improve the problems of low piezoelectric constant and high-temperature resistivity of bismuth calcium titanate ceramics in the related art.
[0006] This application is implemented as follows:
[0007] In a first aspect, an example of the present application provides a piezoelectric ceramic material, the chemical formula of the piezoelectric ceramic material is (1-x)CaBi4Ti4O 15 ·xCa 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6 Ta 2 / 3 ) y NbO9, wherein 0.05≤x≤0.4, 0.1≤y≤0.6.
[0008] In the above implementation process, using Ca 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6 Ta 2 / 3 ) y NbO9 to CaBi4Ti4O 15 Modification and doping can improve the piezoelectric constant and high-temperature resistivity of piezoelectric ceramic materials while maintaining a relatively high Curie temperature, making them suitable for use under high-temperature conditions.
[0009] In combination with the first aspect, in an optional implementation manner of the present application, 0.1≤x≤0.4, 0.2≤y≤0.6.
[0010] In the above implementation process, (1-x)CaBi4Ti4O 15 ·xCa 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6 Ta 2 / 3 ) y In NbO9, 0.1≤x≤0.4, 0.2≤y≤0.6, which can further improve the piezoelectric constant and high temperature resistivity of the piezoelectric ceramic material.
[0011] In a second aspect, the present application example provides a method for preparing the piezoelectric ceramic material provided in the first aspect, comprising:
[0012] Raw materials for forming a piezoelectric ceramic material are weighed according to stoichiometry, the raw materials including CaCO3, Bi2O3, TiO2, Ta2O5, Nb2O5, NiO and ZnO;
[0013] Sintering step: sintering the raw materials to form piezoelectric ceramic materials through solid phase reaction.
[0014] In the above implementation process, CaCO3, Bi2O3, TiO2, Ta2O5, Nb2O5, NiO and ZnO weighed according to stoichiometric amount are solid-phase sintered to obtain a chemical formula of (1-x)CaBi4Ti4O 15 ·xCa 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6Ta 2 / 3 ) y NbO9 piezoelectric ceramic material.
[0015] In combination with the second aspect, in an optional embodiment of the present application, the sintering temperature is 1080-1160° C., and the sintering time is 2-4 hours.
[0016] In the above implementation process, CaCO3, Bi2O3, TiO2, Ta2O5, Nb2O5, NiO and ZnO raw material powders are sintered at a temperature of 1080-1160°C for 2-4 hours to obtain a piezoelectric ceramic material with a higher piezoelectric constant, Curie temperature and high temperature resistivity.
[0017] In combination with the second aspect, in an optional embodiment of the present application, the preparation method further includes a pre-firing step before the sintering step:
[0018] The raw materials are mixed and pre-calcined at 800-950° C. for 2-4 hours to obtain pre-calcined powder.
[0019] Optionally, the heating rate of the pre-burning is 3-5°C / min.
[0020] In the above implementation process, the raw material powder is heated to 800-950° C. and pre-fired for 2-4 hours before sintering, which can improve the piezoelectric properties of the piezoelectric ceramic material obtained by subsequent sintering.
[0021] In combination with the second aspect, in an optional embodiment of the present application, the preparation method further includes a debinding step between the pre-firing step and the sintering step:
[0022] The pre-fired powder and the binder are mixed, ground into granules, sieved and pressed into shape, and then heated to 700-800° C. for debinding sintering for 1-2 hours to obtain a ceramic green body; the sintering step sinters the ceramic green body.
[0023] Optionally, the heating rate of debinding sintering is 1.5-2°C / min.
[0024] Optionally, the binder includes 10 wt % of a PVA aqueous solution, and the PVA aqueous solution accounts for 10% to 15% of the total mass of the pre-calcined powder.
[0025] In the above implementation process, the pre-fired powder is mixed with the PVA binder to form a granulated body for easy pressing into a green body, and then the green body is debinded and sintered to remove the PVA binder to form a ceramic green body. The ceramic green body is sintered to obtain a piezoelectric ceramic material.
[0026] In combination with the second aspect, in an optional embodiment of the present application, the preparation method further includes an electrode sintering step after the sintering step:
[0027] Electrodes are printed on the surface of piezoelectric ceramic material and sintered.
[0028] Optionally, the electrode is a platinum electrode, and the temperature of the sintered electrode is 950° C., and the time is 25 minutes. In conjunction with the second aspect, in an optional embodiment of the present application, the preparation method further includes a polarization treatment step located after the sintering electrode step, the polarization temperature is 170-210° C., the polarization electric field strength is 10-12 kv / mm, and the polarization time is 15-45 minutes.
[0029] In the above implementation process, the piezoelectric ceramic material is polarized at a temperature of 170-210° C. and an electric field strength of 10-12 kv / mm for 15-45 minutes, which can improve the piezoelectric properties of the piezoelectric ceramic material.
[0030] In a third aspect, an example of the present application provides a piezoelectric device, the piezoelectric device comprising the piezoelectric ceramic material provided in the first aspect or a piezoelectric ceramic material prepared according to the method for preparing the piezoelectric ceramic material provided in the second aspect.
[0031] Optionally, the piezoelectric device is a vibration sensor.
[0032] In the above implementation process, the chemical formula is (1-x)CaBi4Ti4O 15 ·xCa 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6Zn 1 / 6 Ta 2 / 3 ) y The piezoelectric devices prepared by the piezoelectric ceramic material of NbO9 can serve at high temperature and have good piezoelectric performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0034] Figure 1 A process flow chart of the preparation of piezoelectric ceramic materials provided for the example of this application;
[0035] Figure 2 A graph showing the change in dielectric constant of the piezoelectric ceramic material provided in Example 2 of the present application as a function of temperature;
[0036] Figure 3 The temperature-piezoelectric constant curve provided for Test Example 2 of this application. DETAILED DESCRIPTION
[0037] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0038] Lead-free bismuth layered structure ceramics have the advantages of high Curie temperature, good temperature stability and environmental friendliness, and are a candidate material suitable for use in high temperature environments.
[0039] Bismuth layered ceramics are made of (Bi2O2) 2+ The chemical formula of the perovskite-like layer is (Bi2O2). 2+ (A m-1 B m O 3m+1 ) 2- Among them, calcium bismuth titanate CaBi4Ti4O 15 Ceramics have the advantages of ideal high Curie point (Tc = 790 ° C) and high depolarization temperature. However, the piezoelectric constant (d 33 ) and 600℃ high temperature resistivity is low, that is, d 33 Only 8pC / N, 600℃ high temperature resistivity 1.1×10 5 Ω·cm, which cannot meet the requirements of high-end piezoelectric devices.
[0040] Therefore, the present application example provides a piezoelectric ceramic material and a preparation method thereof to improve the high-temperature piezoelectric properties of bismuth calcium titanate-based layered structure ceramics.
[0041] The piezoelectric ceramic material provided in the embodiment of the present application has a general chemical formula of (1-x)CaBi4Ti4O 15 ·xCa 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6 Ta 2 / 3 ) y NbO9, wherein 0.05≤x≤0.4, 0.1≤y≤0.6.
[0042] Illustratively, x can be selected from one of 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39 or 0.4, or a range between any two of them.
[0043] Illustratively, y can be selected from one of 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, or a range between any two thereof.
[0044] Exemplarily, x may be selected from 0.05, and y may be selected from 0.1.
[0045] Furthermore, in some possible embodiments, 0.1≤x≤0.4, 0.2≤y≤0.6.
[0046] Exemplarily, x may be selected from 0.1, and y may be selected from 0.5.
[0047] Exemplarily, x may be selected from 0.2, and y may be selected from 0.6.
[0048] Exemplarily, x may be selected from 0.3, and y may be selected from 0.2.
[0049] Exemplarily, x may be selected from 0.4, and y may be selected from 0.2.
[0050] The piezoelectric ceramic material provided in the example of the present application has a piezoelectric constant of not less than 12pC / N, a Curie temperature of not less than 795°C, and a high temperature resistivity of not less than 8.1×10 5 Ω·cm, with good high temperature service performance.
[0051] Furthermore, this application example provides a method for preparing a piezoelectric ceramic material, see Figure 1 ,include:
[0052] S1. Raw materials for forming a piezoelectric ceramic material are weighed according to stoichiometry. The raw materials include CaCO3, Bi2O3, TiO2, Ta2O5, Nb2O5, NiO and ZnO.
[0053] S2, pre-calcining step: the raw materials are mixed and pre-calcined at 800-950° C. for 2-4 hours to obtain pre-calcined powder.
[0054] S3, debinding treatment step: the pre-calcined powder and the binder are mixed, ground into granules, sieved and pressed into shape, and then heated to 700-800°C for debinding sintering for 2 hours to obtain a ceramic green body.
[0055] S4, sintering step: sintering the ceramic green body to form a piezoelectric ceramic material.
[0056] In step S1, CaCO3, Bi2O3, TiO2, Ta2O5, Nb2O5, NiO and ZnO raw materials can be reacted in the solid phase to form Ca 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6 Ta 2 / 3 ) y NbO9 doped calcium bismuth titanate piezoelectric ceramic material, the chemical formula of the piezoelectric ceramic material is (1-x)CaBi4Ti4O 15 ·xCa 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6 Ta 2 / 3 ) y NbO9.
[0057] For example, 99.99% pure CaCO3, 99.99% pure Bi2O3, 99.99% pure TiO2, 99.99% pure Ta2O5, 99.99% pure Nb2O5, 99.99% pure NiO and 99.99% pure ZnO can be selected as raw materials.
[0058] In step S2, the raw materials may be mixed by ball milling.
[0059] Exemplarily, various raw material powders weighed according to the stoichiometric ratio are placed in a ball mill and mixed and ball-milled for 10 hours.
[0060] In step S2, the pre-calcination temperature may be 800°C, 850°C, 900°C, or 950°C, or a range between any two of them.
[0061] In step S2, the pre-burning time may be 2 h, 2.5 h, 3 h or 4 h, or a range between any two of them.
[0062] For example, the pre-sintering may be performed at a temperature of 800° C. for 4 hours.
[0063] For example, the pre-calcination may be performed at 850° C. for 2 h.
[0064] Exemplarily, the pre-calcination may be performed at a temperature of 880° C. for 4 hours.
[0065] Exemplarily, the pre-sintering may be performed at a temperature of 950° C. for 3 hours.
[0066] For example, the heating rate of the pre-firing may be in the range of one or any two of 3° C. / min, 3.5° C. / min, 4° C. / min, 4.5° C. / min or 5° C. / min.
[0067] In step S3, the pre-burned powder obtained in step S2 is mixed with a binder, ground into granules, sieved for pressing and then sintered to increase the sintering rate and the piezoelectric properties of the piezoelectric ceramic material obtained by sintering.
[0068] In a possible embodiment, the adhesive may be selected from a PVA aqueous solution, that is, a polyvinyl alcohol aqueous solution.
[0069] For example, a 10 wt % PVA aqueous solution may be selected.
[0070] Furthermore, in some possible embodiments, the PVA aqueous solution accounts for 10-15% of the total mass of the pre-calcined powder.
[0071] For example, the percentage of the PVA aqueous solution to the total mass of the pre-calcined powder can be 10%, 11%, 12%, 13%, 14% or 15%, or a range between any two of them.
[0072] For example, the pre-calcined powder and the binder are ground and granulated, dried, passed through an 80-mesh sieve, and then pressed into a thin round billet with a diameter of 10 mm and a thickness of 1 mm. The thin round billet is then heated to 700° C., 750° C. or 800° C. for debinding and sintering for 2 hours to obtain a ceramic green billet.
[0073] For example, the heating rate of the debinding treatment may be selected from one of 1.5°C / min, 1.6°C / min, 1.7°C / min, 1.8°C / min, 1.9°C / min or 2.0°C / min, or a range between any two of them.
[0074] In step S4, the ceramic green body may be sintered at a temperature of 1080-1160° C. for 2-4 hours to form a piezoelectric ceramic material.
[0075] Illustratively, the sintering temperature may be one of 1080°C, 1090°C, 1100°C, 1110°C, 1120°C, 1130°C, 1140°C, 1150°C or 1160°C, or a range between any two thereof.
[0076] In step S4, after the ceramic green body is sintered, a sheet-shaped piezoelectric ceramic material can be obtained.
[0077] Furthermore, the method for preparing the piezoelectric ceramic material provided in the example of the present application further includes:
[0078] S5, electrode sintering step: printing electrodes on the surface of the piezoelectric ceramic material and sintering the electrodes.
[0079] By printing and sintering electrodes on the surface of piezoelectric ceramic materials, the current generated by the piezoelectric ceramic materials at the electrode tracks can be utilized, and the piezoelectric ceramic materials can be applied to piezoelectric devices such as vibration sensors.
[0080] In step S5, platinum paste may be printed on the surface of the piezoelectric ceramic material, and then sintered at 950° C. for 10-25 minutes to form a platinum electrode.
[0081] Furthermore, before printing the platinum paste on the surface of the piezoelectric ceramic material, the piezoelectric ceramic material may be polished.
[0082] Furthermore, in order to improve the piezoelectric properties of the piezoelectric ceramic material, the preparation method also includes:
[0083] S6, polarization treatment step: placing the piezoelectric ceramic material in silicone oil and applying voltage for polarization.
[0084] In some possible embodiments, the polarization temperature may be 170-210° C., the polarization electric field intensity may be 10-12 kv / mm, and the polarization time may be 15-45 min.
[0085] For example, the polarization temperature may be in the range of one or any two of 170° C., 180° C., 190° C., 200° C. or 210° C.
[0086] Exemplarily, the electric field strength of the polarization may be in the range of one or any two of 10 kv / mm, 11 kv / mm or 12 kv / mm.
[0087] Exemplarily, the polarization time may be in the range of one or any two of 15 min, 20 min, 25 min, 30 min, 35 min, 40 min or 45 min.
[0088] Furthermore, the present application example provides a piezoelectric device, including the piezoelectric ceramic material provided in the present application example.
[0089] Illustratively, the present application provides a vibration sensor, which includes a piezoelectric ceramic material, and a counterweight is provided on an electrode of the piezoelectric ceramic material.
[0090] The piezoelectric ceramic material of the present application is further described in detail below in conjunction with the embodiments.
[0091] Example 1
[0092] Embodiment 1 provides a piezoelectric ceramic material, and the preparation method is as follows:
[0093] Step (1):
[0094] According to 0.95CaBi4Ti4O 15 0.05Ca 0.05 Bi 2.97 Ti 0.9 (Ni 1 / 6 Zn 1 / 6 Ta 2 / 3 ) 0.1 The stoichiometric ratio of NbO9 (i.e. x=0.05, y=0.1) is adopted, and the raw materials of CaCO3 (99.99% purity), Bi2O3 (99.99% purity), TiO2 (99.9% purity), ZnO (99% purity), NiO (99% purity), Ta2O5 (99.99% purity), and Nb2O5 (99.99% purity) are weighed.
[0095] Step (2): The raw materials obtained in step (1) are placed in a ball mill and mixed and ball milled for 10 hours, and pre-calcined at 800° C. for 3 hours at a heating rate of 3° C. / min.
[0096] Step (3): The pre-fired powder obtained in step (2) is ball-milled for a second time for 48 hours. After the material is dried, a 10 wt% PVA aqueous solution is added, which is about 15% of the weight of the pre-fired powder. The mixture is evenly mixed and then sieved through an 80-mesh sieve. The mixture is pressed into a thin round billet with a diameter of 10 mm and a thickness of 1 mm. The powder is subjected to a binder removal treatment at 800°C for 2 hours to remove the PVA and obtain a ceramic blank.
[0097] Step (4): The ceramic blank obtained in step (3) is sintered at 1120° C. for 3 hours to obtain a ceramic sheet.
[0098] Step (5): polish both sides of the ceramic sheet obtained in step (4), print platinum electrodes, and keep the temperature at 950° C. for 25 minutes.
[0099] Step (6): Place the ceramic sheet in 170°C silicone oil and apply a DC electric field of 12 kV / mm for 35 min.
[0100] Example 2
[0101] Embodiment 2 provides a piezoelectric ceramic material, which differs from Embodiment 1 in that:
[0102] In step (1), x=0.1, y=0.5.
[0103] In step (2), the pre-firing temperature is 800°C, the pre-firing time is 3h, and the heating rate is 4°C / min.
[0104] In step (3), the weight of the PVA aqueous solution is about 10% of the pre-calcined powder.
[0105] In step (4), the ceramic blank is sintered at 1080° C. for 4 hours.
[0106] In step (6), the ceramic sheet is placed in 210° C. silicone oil and a DC electric field of 12 kV / mm is applied and maintained for 45 minutes.
[0107] Example 3
[0108] Embodiment 3 provides a piezoelectric ceramic material, which differs from Embodiment 1 in that:
[0109] In step (1), x=0.2, y=0.6.
[0110] In step (2), the pre-firing temperature is 950°C, the pre-firing time is 4h, and the heating rate is 5°C / min.
[0111] In step (4), the ceramic blank is sintered at 1160° C. for 2 hours.
[0112] In step (6), the ceramic sheet is placed in silicone oil at 170° C. and a DC electric field of 12 kV / mm is applied and maintained for 25 minutes.
[0113] Example 4
[0114] Embodiment 4 provides a piezoelectric ceramic material, which differs from Embodiment 1 in that:
[0115] In step (1), x=0.3, y=0.2.
[0116] In step (2), the pre-firing temperature is 850°C, the pre-firing time is 4h, and the heating rate is 3°C / min.
[0117] In step (3), the weight of the PVA aqueous solution is about 10% of the pre-calcined powder.
[0118] In step (4), the ceramic blank is sintered at 1110° C. for 4 hours.
[0119] In step (6), the ceramic sheet is placed in 210° C. silicone oil and a DC electric field of 12 kV / mm is applied and maintained for 45 minutes.
[0120] Example 5
[0121] Embodiment 5 provides a piezoelectric ceramic material, which is different from Embodiment 1 in that:
[0122] In step (1), x=0.4, y=0.2.
[0123] In step (2), the pre-firing temperature is 800°C, the pre-firing time is 4h, and the heating rate is 3°C / min.
[0124] In step (3), the weight of the PVA aqueous solution is about 10% of the pre-calcined powder.
[0125] In step (4), the ceramic blank is sintered at 1160° C. for 3 hours.
[0126] In step (6), the ceramic sheet is placed in silicone oil at 170° C. and a DC electric field of 12 kV / mm is applied and maintained for 25 minutes.
[0127] Example 6
[0128] Example 6 provides a piezoelectric ceramic material, which differs from Example 2 in that, in step (2), the pre-firing temperature is 700° C., the pre-firing time is 3 h, and the heating rate is 4° C. / min.
[0129] Comparative Example 1
[0130] The difference between Comparative Example 1 and Example 2 is that:
[0131] In step (1), the piezoelectric ceramic material is not doped, and the chemical formula of the piezoelectric ceramic material is CaBi4Ti4O 15 The raw materials do not contain ZnO, NiO, Ta2O5, and Nb2O5.
[0132] Comparative Example 2
[0133] The difference between Comparative Example 2 and Example 1 is:
[0134] In step (1), NiO in the raw material is replaced by Yb2O3 (99.99% purity).
[0135] Comparative Example 3
[0136] The difference between Comparative Example 3 and Example 1 is that:
[0137] In step (1), ZnO in the raw material is replaced by CeO2 (99% purity).
[0138] Comparative Example 4
[0139] The difference between Comparative Example 4 and Example 1 is that:
[0140] In step (1), ZnO and NiO in the raw materials are replaced by Yb2O3 (99% purity) and CeO2 (99% purity).
[0141] Test Example 1
[0142] The piezoelectric performance of the piezoelectric ceramic materials provided in Examples 1-6 and Comparative Examples 1-4 was tested in the following manner:
[0143] The test results are shown in Table 1. The dielectric constant of the piezoelectric ceramic material provided in Example 2 varies with temperature. Figure 2 shown.
[0144] Table 1
[0145]
[0146] Test Example 2
[0147] The piezoelectric ceramic materials provided in Examples 1-6 and Comparative Examples 1-4 were annealed in the temperature range of 150-750° C., kept at each temperature for 2 hours, and the piezoelectric constants were tested. The test results are as follows: Figure 3 shown.
[0148] Result analysis:
[0149] Combined with Table 1, Figure 2 and Figure 3 The raw materials of Comparative Examples 1-4 do not contain ZnO, NiO, Ta2O5 and Nb2O5, and the Curie temperature of the obtained piezoelectric ceramic material does not exceed 792°C, the piezoelectric constant does not exceed 11pC / N, and the high temperature resistivity at 600°C does not exceed 9.2×10 5 Ω·cm; and in Examples 1-6 of the present application, using Ca 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6 Ta 2 / 3 ) y NbO9 to CaBi4Ti4O 15 Modification and doping were performed to obtain the chemical formula (1-x)CaBi4Ti4O 15 ·xCa 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6Ta 2 / 3 ) y The piezoelectric ceramic material of NbO9, 0.05≤x≤0.4, 0.1≤y≤0.6 can increase the piezoelectric constant to not less than 12.0pC / N and the high temperature resistivity to not less than 8.1×10 5 Ω·cm. This indicates that the piezoelectric ceramic materials provided in Examples 1 to 6 of the present application can improve the high-temperature resistivity and piezoelectric constant at 600° C. while maintaining a relatively high Curie temperature.
[0150] And, from Figure 3 It can be seen that after the piezoelectric ceramic material provided in Example 2 is annealed at 600°C for 2h, its piezoelectric constant d 33 It can still reach 23.5pC / N, with higher piezoelectricity and temperature stability.
[0151] By comparing Example 2 and Example 6, it can be seen that the piezoelectric performance of the piezoelectric ceramic material obtained by pre-firing Example 6 at a temperature of 700°C is lower than that of Example 2, indicating that Example 2 of the present application is pre-firing at a temperature of 800-950°C for 2-4h, which can further improve the piezoelectric performance of the piezoelectric ceramic material. The above description is only a preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A piezoelectric ceramic material, characterized in that: The chemical formula of the piezoelectric ceramic material is (1-x)CaBi4Ti4O 15 ·xCa 0.05 Bi 2.97 Ti 1-y (Ni 1 / 6 Zn 1 / 6 Ta 2 / 3 ) y NbO9, wherein 0.05≤x≤0.4, 0.1≤y≤0.
6.
2. The piezoelectric ceramic material according to claim 1, characterized in that: 0.1≤x≤0.4, 0.2≤y≤0.
6.
3. A method for preparing a piezoelectric ceramic material according to claim 1 or 2, characterized in that: include: Weigh raw materials for forming the piezoelectric ceramic material according to stoichiometry, the raw materials including CaCO3, Bi2O3, TiO2, Ta2O5, Nb2O5, NiO and ZnO; Sintering step: sintering the raw materials to form the piezoelectric ceramic material through solid phase reaction.
4. The preparation method according to claim 3, characterized in that: The sintering temperature is 1080-1160° C. and the sintering time is 2-4 hours.
5. The preparation method according to claim 4, characterized in that: The preparation method further comprises a pre-firing step before the sintering step: The raw materials are mixed and pre-calcined at 800-950° C. for 2-4 hours to obtain a pre-calcined powder; Optionally, the heating rate of the pre-burning is 3-5°C / min.
6. The preparation method according to claim 5, characterized in that: The preparation method further comprises a debinding step between the pre-sintering step and the sintering step: The pre-calcined powder and the binder are mixed, ground into granules, sieved and pressed into shape, and then heated to 700-800° C. for debinding and sintering for 1-2 hours to obtain a ceramic green body; Optionally, the heating rate of the debinding sintering is 1.5-2°C / min.
7. The preparation method according to claim 6, characterized in that: The binder comprises 10 wt% of a PVA aqueous solution, and the PVA aqueous solution accounts for 10% to 15% of the total mass of the pre-calcined powder.
8. The preparation method according to claim 7, characterized in that: The preparation method further comprises an electrode sintering step after the sintering step: Printing electrodes on the surface of the piezoelectric ceramic material and sintering the electrodes; Optionally, the electrode is a platinum electrode, and the sintering temperature of the electrode is 950° C. and the time is 25 minutes.
9. The preparation method according to claim 8, characterized in that: The preparation method further comprises a polarization treatment step after the electrode sintering step, wherein the polarization temperature is 170-210° C., the polarization electric field intensity is 10-12 kv / mm, and the polarization time is 15-45 min.
10. A piezoelectric device, characterized in that: The piezoelectric device comprises the piezoelectric ceramic material according to claim 1 or 2 or the piezoelectric ceramic material prepared according to the preparation method according to any one of claims 3 to 9; Optionally, the piezoelectric device is a vibration sensor.
Citation Information
Patent Citations
Piezoelectric ceramic material, preparation method thereof and piezoelectric device
CN116606137A
Bi.Na.Ag Ba titanate series lead-free piezoelectric ceramics
CN1814569A
Bi.Na.K.Li Ag titanate series lead-free piezoelectric ceramics
CN1814570A
Piezoelectric ceramic material with high bulk resistivity and laminated bismuth structure and its preparing method
CN1986485A
Crystal-oriented ceramic and its manufacturing method
JP2004300019A