TGO-corrosion-resistant HfSiO4 bonding layer material with coating type microstructure for EBC and preparation method and application of TGO-corrosion-resistant HfSiO4 bonding layer material
Through wet ball milling and high-temperature sintering of HfO2 powder and silicon sol, a microstructure of HfSiO4 coated HfO2 is formed, which solves the problems of TGO corrosion and oxygen conductivity in SiC/SiC composite materials, and achieves improved heat resistance and stability.
Patent Information
- Application Number
- CN202411141829.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The Si and Si-HfO2 bonding layers commonly used in the environmental barrier coating (EBC) of SiC/SiC composites are easily oxidized to form thermally grown oxides (TGO), resulting in cracks, stratification and failure, and the oxygen conductivity of HfO2 is not favorable. To prevent oxygen diffusion, the HfSiO4 bonding layer is difficult to fully synthesize the solid phase at high temperatures, and micropores and oxygen conductivity residues are easily generated.
Wet ball milling was performed using HfO2 powder and silica sol at a ratio of 1:0.8 to 1.6 to form a nano-scale SiO2-coated HfO2 structure. After high temperature sintering, a microstructure of HfSiO4-coated HfO2 was obtained to form a heat-resistant growth Oxide (TGO)-corroded HfSiO4 bonding layer material for EBC with a coated microstructure.
It delays the mass transfer process of TGO, improves the stability and service life of the EBC system, maintains the thermal expansion matching with SiC/SiC composite materials, reduces oxygen diffusion, and enhances the anti-drying air oxidation performance.
Smart Images

Figure CN118930256A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of SiC ceramic-based composite materials, and in particular to a HfSiO4 bonding layer for EBC with a coating-type microstructure and resistant to heat grown oxide (TGO) corrosion, and a preparation method and application thereof. Background Art
[0002] SiC / SiC composites are ideal high-temperature structural materials for aircraft engines. The high temperature, corrosion, gas scouring and other multi-factor interactive environments of aircraft engines cause the surface stability of SiC / SiC composites to deteriorate sharply. Environmental barrier coatings (EBCs) can establish a barrier between SiC / SiC composites and the harsh environment of the engine, thereby preventing or weakening the impact of the engine environment on high-temperature structural materials as much as possible.
[0003] Similar to thermal barrier coatings (TBCs), EBCs also require an adhesive layer, which serves as a link between the upper and lower layers. On the one hand, it can improve the bonding strength between the EBC surface layer and the SiC / SiC substrate, and on the other hand, it can prevent oxygen or water vapor from further diffusing through the EBC surface layer. It is an important component of the EBC system. So far, SiC / SiC composite EBCs often use Si, Si-HfO2, etc. as adhesive layers. However, the Si adhesive layer is easily oxidized to form thermally grown oxides (TGO, here refers to SiO2), which form cracks and lead to EBC delamination, peeling, and failure. The Si-HfO2 bonding layer is a Si bonding layer modified with HfO2 (up to 2800°C) with a higher melting point, which can improve the creep strength and high-temperature performance of the bonding layer. At the same time, HfO2 and Si are oxidized to generate HfSiO4 at high temperatures, and the thermal expansion coefficient of HfSiO4 itself is closer to that of SiC / SiC composite materials, which will not cause CTE mismatch; HfSiO4 has a lower oxygen diffusion coefficient, which effectively reduces the penetration of oxygen into the base material and inhibits the generation of TGO; secondly, the thermal expansion coefficient can be adjusted using the ratio of Si / HfO2. However, HfO2 itself is a good conductor of oxygen, which is not conducive to hindering the diffusion of oxygen into the base material; it is difficult to accurately control the amount of HfO2 doping, and Si has the risk of continued oxidation.
[0004] Therefore, some researchers have proposed to use HfSiO4 directly as a bonding layer, but there are chemical reaction limitations: due to thermodynamic and kinetic limitations, it is difficult to completely solid-phase synthesize HfSiO4 in a 1:1 ratio during subsequent heat treatment using the spraying raw materials HfO2 and SiO2; the heat treatment time is too long (up to hundreds of hours) and micropores are easily generated; and residual HfO2 is a good conductor of oxygen, which is not conducive to hindering the diffusion of oxygen into the base material.
[0005] To this end, the present invention provides an improved solution to prepare a HfSiO4 bonding layer material for EBC that is resistant to TGO corrosion and has a coated microstructure. Summary of the invention
[0006] In order to solve the above-mentioned deficiencies in the prior art, the present invention provides a HfSiO4 bonding layer material for EBC with a coated microstructure that is resistant to TGO corrosion, and a preparation method and application thereof.
[0007] The first object of the present invention is to provide a method for preparing a HfSiO4 bonding layer material for EBC with a coating type microstructure and resistant to TGO corrosion, comprising the following steps:
[0008] S1. Mix HfO2 powder and silica sol at a Hf:Si molar ratio of 1:0.8 to 1.6, and then perform wet ball milling to obtain a slurry; dry the slurry and grind it to obtain a mixed powder;
[0009] S2. The mixed powder is sintered at a high temperature of 1450-1600° C. and then ground into powder to obtain a TGO corrosion-resistant EBC HfSiO4 bonding layer material with a coated microstructure.
[0010] Preferably, the purity of the HfO2 powder is ≥99.99wt.%; and / or the particle size of the HfO2 powder is 3-6μm.
[0011] Preferably, the purity of the silica sol is 25 wt.%; and / or the particle size of SiO2 in the silica sol is 8 to 12 μm.
[0012] Preferably, the ball milling aid of the wet ball milling is anhydrous ethanol, the ball milling rate is 20 to 60 Hz, and the ball milling time is 12 to 24 hours.
[0013] Preferably, the drying temperature of the slurry is 60-80° C., and the drying time is 12-24 hours.
[0014] Preferably, the grinding condition of the slurry after drying is an agate mortar, and the grinding time is 20 to 40 minutes.
[0015] Preferably, the particle size of the slurry after drying and grinding is 10 to 15 μm.
[0016] Preferably, the high-temperature sintering time of the mixed powder is 1 to 5 hours.
[0017] Preferably, after the high-temperature sintering, the grinding condition is an agate mortar, and the grinding time is 30 to 50 minutes.
[0018] Preferably, the particle size of the powder after high-temperature sintering and grinding is 40 to 70 μm.
[0019] Another object of the present invention is to provide a HfSiO4 bonding layer material prepared by the above method.
[0020] Another object of the present invention is to improve the application of a HfSiO4 bonding layer material in the preparation of HfSiO4 bonding layers.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention uses HfO2 powder and silica sol as raw materials to synthesize HfSiO4, so as to maintain the good performance of thermal expansion matching between the environmental barrier coating material and the SiC / SiC composite material through the synthesis of HfSiO4, and forms a coated structure after ball milling and mixed sintering, so as to effectively delay the mass transfer process of TGO, thereby delaying the fragmentation and shedding of the entire EBC system.
[0023] The process flow of the invention is simple, the process feasibility is high, and the raw materials are easily available. In addition, the bonding layer material prepared by the invention is resistant to TGO corrosion, has a thermal expansion coefficient similar to that of SiC / SiC composite materials, has an adjustable thermal expansion coefficient, and has excellent resistance to dry air oxidation. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A schematic diagram of the microstructure of the bonding layer formed by the bonding layer material prepared by the present invention;
[0025] Figure 2 The XRD patterns of the coated powder of the present invention measured at different ratios (Hf:Si);
[0026] Figure 3 The XRD patterns of the coated powder of the present invention measured at different sintering temperatures;
[0027] Figure 4 The XRD spectrum of the uncoated powder prepared in Comparative Example 1;
[0028] Figure 5 TEM image of the uncoated powder prepared in Comparative Example 1;
[0029] Figure 6 The XRD spectrum of Comparative Example 1 measured before and after SiO2 corrosion;
[0030] Figure 7 The XRD spectrum of Example 1 measured before and after SiO2 corrosion;
[0031] Figure 8 This is the TEM image of the coated powder prepared in Example 1. DETAILED DESCRIPTION
[0032] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0033] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.
[0034] As described in the background technology, the common Si bonding layer has a low melting point, poor temperature resistance, and poor oxidation resistance and water-oxygen corrosion resistance; the temperature resistance of the Si-HfO2 bonding layer is certainly improved, but the existing Si component still has the risk of being oxidized and corroded by water and oxygen, and HfO2 itself is a good conductor of oxygen, which is not conducive to hindering the diffusion of oxygen into the matrix material. In addition, it is difficult to accurately control the amount of HfO2 doping; the HfSiO4 bonding layer recently proposed by researchers has the problem of easily causing micropores inside the bonding layer, too long post-processing time, and also residual HfO2, which is not conducive to hindering the diffusion of oxygen into the matrix material.
[0035] Based on this, the present invention uses silica sol as the raw material for preparation, forms a structure of nano-scale SiO2 coated HfO2 by ball milling, and obtains a microstructure of HfSiO4 coated HfO2 after high-temperature sintering. On the one hand, after HfSiO4 is coated with HfO2, the contact between HfO2 and TGO (SiO2) can be inhibited, thereby improving the corrosion barrier effect of the raw materials of the bonding layer on TGO; on the other hand, the excellent properties of HfSiO4 itself are retained, that is, the thermal expansion coefficient is similar to that of SiC / SiC composite materials, and the oxygen diffusion coefficient is low; in addition, the overall thermal expansion coefficient of the bonding layer can be adjusted by adjusting the ratio of silica sol and HfO2. The technical scheme in the embodiment of the present invention will be described clearly and completely below:
[0036] Step 1, mix the raw materials:
[0037] The HfO2 powder and silica sol are mixed at a molar ratio of HfO2 powder to SiO2 of 1:0.8-1.6, and then wet ball milling is performed to obtain a slurry; the slurry is dried and then ground to obtain a mixed powder.
[0038] It should be noted that the present invention uses silica sol and HfO2 powder as raw materials to synthesize HfSiO4, so as to maintain the good thermal expansion matching performance of the environmental barrier coating material and the SiC / SiC composite material by synthesizing a certain amount of HfSiO4, and on the basis of ensuring that the prepared environmental barrier coating material and the SiC / SiC composite material have good thermal expansion matching, a coating structure is formed to further improve the barrier effect of the bonding layer raw material against TGO corrosion.
[0039] In order to ensure that the overall thermal expansion coefficient of the environmental barrier coating material finally prepared by the present invention still maintains a good match with the SiC / SiC composite material, in a preferred scheme of the present invention, HfO2 powder and silica sol are first premixed, and then anhydrous ethanol is used as a ball milling aid to perform wet ball milling on the premixed HfO2 powder and silica sol mixture, so that the HfO2 powder and SiO2 powder are fully mixed and form a coating structure. The preferred wet ball milling rate is 20-60Hz, and the ball milling time is 12-24h.
[0040] In order to further promote the full mixing of HfO2 and SiO2, in a preferred embodiment of the present invention, HfO2 is preferably added in the form of high-purity powder, and silica sol SiO2 is added in the form of liquid. The purity of HfO2 powder is ≥99.99wt.%; the particle size of HfO2 powder is 3-6μm. The purity of silica sol is 25wt.%; the particle size of SiO2 in silica sol is 8-12μm.
[0041] In order to facilitate subsequent high-temperature sintering treatment, in a preferred embodiment of the present invention, the slurry after wet ball milling is also dried to remove excess anhydrous ethanol, and the drying temperature is 60-80°C and the drying time is 12-24h.
[0042] In order to prevent the material from agglomerating during the drying process, which is not conducive to high-temperature sintering, the dried product is ground before high-temperature sintering, so that the mixed powder can be fully calcined in an air atmosphere during the high-temperature sintering process. However, in order to prevent other impurities from entering during grinding and avoid affecting the next step of high-temperature solid-phase reaction, the grinding time cannot be long. In a preferred embodiment of the present invention, the grinding time is 20 to 40 minutes.
[0043] In order to avoid the incorporation of other impurities during the grinding process, which is not conducive to the purity of the raw materials of the generated bonding layer, the mortar used in the grinding process is preferably an agate mortar. The component of the agate mortar is SiO2, which can preferably avoid the incorporation of other impurities.
[0044] Step 2, high temperature sintering:
[0045] The mixed powder is sintered at high temperature and ground into powder, so as to obtain a TGO corrosion-resistant HfSiO4 bonding layer material for EBC with a coating type microstructure.
[0046] It should be noted that the present invention takes into account the fact that solid-phase reactions generally have low activity, and sufficient activation energy is required before the reaction begins, and the solid-phase reaction rate is slow and requires sufficient time to react. In a preferred embodiment of the present invention, the sintering temperature of the high-temperature sintering is 1450-1600°C, and the sintering time is 1-5h, so as to achieve the purpose of high purity and uniformity of the final product.
[0047] The HfSiO4 bonding layer material for EBC with a coated microstructure and resistant to TGO corrosion obtained by the present invention ultimately contains HfSiO4 and HfO2.
[0048] In order to allow those skilled in the art to further understand the technical solution of the present invention, the technical solution of the present invention is further described in detail below through specific embodiments and comparative examples.
[0049] Comparative Example 1:
[0050] This comparative example provides a HfSiO4 bonding layer material for EBC without a coating type microstructure, and its preparation method is as follows:
[0051] 1) Using HfO2 powder with a particle size of 6 μm and a purity of 99.99 wt.%, and SiO2 powder with a particle size of 8 μm and a purity of 99.99 wt.% as preparation raw materials, according to the equal molar ratio of Hf:Si, weigh the corresponding masses of the above HfO2 powder and SiO2 powder respectively, and set them aside.
[0052] 2) The weighed HfO2 powder and SiO2 powder are mixed to obtain a mixed material; an equal amount of anhydrous ethanol is added to the mixed material as a ball milling aid, and the mixture is ball milled at a ball milling speed of 40 Hz for 20 hours to obtain a slurry.
[0053] 3) The slurry obtained above was dried in an oven at 70° C. for 24 h, and the dried slurry was ground in an agate mortar for 30 min to obtain a mixed powder, and the powder particle size after grinding was about 14 μm.
[0054] 4) The mixed powder obtained above was sintered at 1500°C for 2h in an air atmosphere, and the mixed powder after high-temperature sintering was ground in an agate mortar for 40min. The powder particle size after grinding was about 58μm, and the HfSiO4 bonding layer material for EBC with a coated microstructure resistant to TGO corrosion of the present invention was obtained as a comparison material.
[0055] Example 1: (The only difference from Comparative Example 1 is that SiO2 powder is replaced by silica sol)
[0056] This embodiment provides a HfSiO4 bonding layer material for EBC with a coated microstructure and resistant to TGO corrosion, and the preparation method thereof is as follows:
[0057] 1) Using HfO2 powder with a particle size of 6 μm and a purity of 99.99 wt.%, and silica sol (with water as solvent) with a particle size of 8 μm and a purity of 25 wt.% as preparation raw materials, according to the Hf:Si molar ratio of 1:1, weigh the corresponding masses of the above HfO2 powder and silica sol respectively, and set them aside.
[0058] 2) The weighed HfO2 powder and silica sol are mixed to obtain a mixed material; an equal amount of anhydrous ethanol is added to the mixed material as a ball milling aid, and the mixture is ball milled at a ball milling speed of 40 Hz for 20 hours to obtain a slurry.
[0059] 3) The slurry obtained above was dried in an oven at 70° C. for 24 h, and the dried slurry was ground in an agate mortar for 30 min to obtain a mixed powder, and the powder particle size after grinding was about 14 μm.
[0060] 4) The mixed powder obtained above is sintered at 1500°C for 2 hours in an air atmosphere, and the high-temperature sintered body is ground in an agate mortar for 40 minutes. The powder particle size after grinding is 58 μm, thus obtaining the HfSiO4 bonding layer material for EBC with a TGO corrosion-resistant coated microstructure of the present invention.
[0061] Embodiment 2:
[0062] The only difference between this embodiment and embodiment 1 is that the molar ratio of Hf:Si in step 1) is replaced with 1:0.8, and the rest remains the same.
[0063] Embodiment 3:
[0064] The difference between this embodiment and embodiment 1 is that the molar ratio of Hf:Si in step 1) is replaced with 1:1.8, and the rest remains the same.
[0065] Embodiment 4:
[0066] The only difference between this embodiment and embodiment 1 is that the sintering temperature in step 3) is replaced with 1300° C., and the rest remain the same.
[0067] Embodiment 5:
[0068] The difference between this embodiment and embodiment 1 is that the sintering temperature in step 3) is replaced with 1450° C., and the rest remain the same.
[0069] Embodiment 6:
[0070] The only difference between this embodiment and embodiment 1 is that the sintering temperature in step 3) is replaced with 1600° C., and the rest remain the same.
[0071] 1. TEM tests were performed on Example 1 and Comparative Example 1. The results are as follows: Figure 5 and Figure 8 As shown, Figure 5 TEM images of the uncoated powder prepared in Comparative Example 1, wherein Figure (a) is a microscopic schematic diagram of the uncoated powder, Figure (b) is a Hf element distribution diagram, Figure (c) is a Si element distribution diagram, and Figure (d) is an O element distribution diagram; Figure 8 TEM images measured for coated powders, where (a) is a microscopic schematic diagram of the coated powder, (b) is the Hf element distribution diagram, (c) is the Si element distribution diagram, (d) is the O element distribution diagram, (e) is a partial enlarged diagram of (a), (f) is a partial enlarged diagram of (e), (j) is the lattice fringe spacing of HfSiO4 and HfO2, and (k) is the diffraction spot of HfSiO4. Figure 5 The results show that the HfSiO4 in Comparative Example 1 is a flake structure and does not have a coating structure. Figure 8 The results (f) show that in the HfSiO4 in Example 1, it can be clearly observed that HfO2 is embedded in the interior of HfSiO4, thus forming a coated structure.
[0072] Furthermore, in order to verify that the synthesized powder has a coated structure, SiO2 corrosion experiments were also carried out on Example 1 and Comparative Example 1. The synthesized powder and high-purity SiO2 were ground and mixed in a mortar, and the molar ratio of synthetic powder: SiO2 = 1:2 was used, and then placed in a BN crucible for corrosion, and XRD tests were performed before and after corrosion. The results are as follows: Figure 4 , Figure 6 , Figure 7 As shown, Figure 4 This is the XRD pattern of the synthesized uncoated HfSiO4 type. Figure 6 This is the XRD spectrum of the uncoated powder before and after SiO2 corrosion. Figure 7 The XRD patterns of coated powders before and after SiO2 corrosion are shown in Figure 2. Figure 6 and Figure 7 By comparison, there is no residual HfO2 in Comparative Example 1 after SiO2 corrosion, while there is still residual HfO2 in Example 1 after SiO2 corrosion, which shows that the synthesized powder has a coated structure, and this coated structure is resistant to TGO corrosion. During the corrosion process, the coated structure will delay the mass transfer process of TGO, thereby delaying the shedding and fragmentation process of the entire EBC system, greatly improving the service life of EBC.
[0073] 2. Verify the effect of different molar ratios (Hf:Si) on the product;
[0074] In order to verify the effect of different molar ratios (Hf:Si) on the product, based on Example 1, only the molar ratio of Hf:Si was changed, and Hf:Si=1:0.8-1.6 was selected to synthesize HfSiO4 and the coated HfSiO4 was tested by XRD. The test results are as follows: Figure 4 As shown, from Figure 4 It can be seen that in the present invention, as the Hf:Si ratio decreases, when the ratio is greater than 1.6, there will be residual SiO2. It can be seen that the molar ratio of Hf:Si must be controlled within 1.6 to effectively make the reaction complete, thereby achieving the purpose of no residual SiO2, improving the purity and preparation efficiency of HfSiO4, and reducing the preparation cost. When Hf:Si<0.8, there will be a large amount of residual HfO2, which will aggravate the corrosion of oxygen elements to the bonding layer material; when Hf:Si>1.6, there will be residual SiO2, and the residual SiO2 will accelerate the generation of thermally grown oxides of the bonding layer material, thereby aggravating the shedding of the entire EBC.
[0075] 3. Verify the influence of different sintering temperatures on the product
[0076] In order to verify the effect of different sintering temperatures on the product, based on Example 1, only the sintering temperature was changed, and a temperature range of 1450-1600°C was selected to synthesize HfSiO4 and an XRD test was performed on the synthesized HfSiO4. The test results are as follows: Figure 5 As shown, Figure 5 The XRD patterns of the products are shown in Figure 2. Figure 5 It can be seen that when the sintering temperature is less than 1450°C, there will be residual SiO2 in the product. This is because there is not enough activation energy provided in the solid phase reaction to support the reaction, resulting in incomplete reaction of HfO2 and SiO2, and the purity of the generated HfSiO4 is not high. From this phenomenon, it can be seen that the reaction needs to be above 1450°C to complete the reaction. However, too high a temperature (over 1600°C) will cause increased energy consumption, increased production costs and increased equipment loss, as well as accelerate the growth rate of the crystal, resulting in structural instability, thereby affecting the physical properties and chemical stability of the material. Therefore, the preferred temperature range of the present invention is 1450-1600°C.
[0077] In order to verify the feasibility of using the powder material synthesized by the present invention for the bonding layer of SiC / SiC composite materials, 20 g of the environmental barrier coating materials prepared in the above Examples 1-6 and Comparative Example 1 were placed in a graphite mold, and hot-pressed and sintered for 2 hours in a vacuum hot-pressing furnace at 1500°C / 35MPa to prepare block ceramics corresponding to Examples 1-6 and Comparative Example 1.
[0078] The thermal expansion coefficient ɑ (25-1600°C), the mass change rate Δm1 after 100h of dry air treatment at 1500°C, and the mass change rate Δm2 after 100h of water-oxygen corrosion at 1300°C of the block ceramics corresponding to the above-obtained Examples 1-6 and Comparative Example 1 were tested respectively, and the structures are shown in Table 1.
[0079] Table 1
[0080]
[0081] It can be seen from the test results in Table 1 that the environmental barrier coating bonding layer materials prepared in Examples 1, 2, 3, 5, and 6 are significantly improved compared with the uncoated HfSiO4 material prepared in Comparative Example 1 after being treated with dry air at 1500°C for 100 hours and with water and oxygen corrosion at 1300°C for 100 hours, and the generated HfSiO4 has a suitable CTE value (matching the SiC / SiC composite material), and in the EBC, water vapor and oxygen can penetrate through the top and middle coatings and react with the SiC matrix to form a TGO layer. The HfSiO4 with a coated structure can effectively delay the mass transfer process of TGO, thereby delaying the fragmentation and shedding of the entire EBC system.
[0082] It can be seen from the test results in Table 1 that, compared with Comparative Example 1, the thermal expansion coefficients of the bonding layer materials of Examples 1, 2, 5, and 6 are still well matched with the SiC / SiC composite material; the mass change after 1500°C dry air treatment for 100 hours is extremely small, almost zero, indicating that Example 1 has excellent anti-drying oxidation performance; the mass change rate after 1300°C water-oxygen corrosion for 100 hours is lower than that of the uncoated HfSiO4, indicating that the water-oxygen corrosion resistance of the coated HfSiO4 has been greatly improved, but the water-oxygen corrosion resistance of Example 3 is slightly worse than that of Examples 1, 2, 5, and 6. This is because the Hf:Si ratio is too small, resulting in residual SiO2 in the reaction product, and the residual SiO2 will cause reaction with water vapor and oxygen to form TGO, aggravating the corrosion of the bonding layer material, but the overall water-oxygen corrosion resistance and air-drying resistance are greatly improved compared with the comparative example, which shows that the coated structure has a significant effect. However, in Example 4, HfSiO4 was not generated during the sintering process at 1300°C. This is because the sintering temperature was too low and did not provide sufficient activation energy to support the reaction. The reaction products were all unreacted SiO2 and HfO2, both of which have excellent resistance to high-temperature oxidation. Their quality did not change much under dry air treatment at 1500°C. However, under water-oxygen corrosion at 1300°C, the residual SiO2 in the bonding layer material would react with water vapor and oxygen to form TGO, aggravating the corrosion of the bonding layer material, thereby aggravating the weight loss of the bulk ceramic. Therefore, the weight loss due to water-oxygen corrosion was the largest in Example 4.
[0083] As an application of HfSiO4 bonding layer material, the HfSiO4 bonding layer formed on the surface of SiC / SiC composite material has a microstructure such as Figure 1 The methods for forming the bonding layer include atmospheric plasma spraying, physical vapor deposition, slurry coating, etc., which are conventional techniques in the art and will not be described one by one here.
[0084] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing a HfSiO4 bonding layer material for EBC with a coating type microstructure and resistant to TGO corrosion, characterized in that: The following steps are involved: S1. Mix HfO2 powder and silica sol at a Hf:Si molar ratio of 1:0.8 to 1.6, and then perform wet ball milling to obtain a slurry; dry the slurry and grind it to obtain a mixed powder; S2. The mixed powder is sintered at a high temperature of 1450-1600° C. and then ground into powder to obtain a TGO corrosion-resistant EBC HfSiO4 bonding layer material with a coated microstructure.
2. The preparation method according to claim 1, characterized in that The HfO2 powder and silica sol are mixed at a Hf:Si molar ratio of 1:1 to 1.
2.
3. The preparation method according to claim 1, characterized in that: The purity of the HfO2 powder is ≥99.99wt.%; and / or the particle size of the HfO2 powder is 3-6μm.
4. The preparation method according to claim 1, characterized in that: The purity of the silica sol is 25 wt.%; and / or the particle size of SiO2 in the silica sol is 8 to 12 μm.
5. The preparation method according to claim 1, characterized in that: The ball milling aid of the wet ball milling is anhydrous ethanol, the ball milling rate is 20 to 60 Hz, and the ball milling time is 12 to 24 hours.
6. The preparation method according to claim 1, characterized in that: The drying temperature of the slurry is 60-80° C., and the drying time is 12-24 hours.
7. The preparation method according to claim 1, characterized in that: In step S1, the grinding condition is an agate mortar, and the grinding time is 20 to 40 minutes; in step S2, the grinding condition is an agate mortar, and the grinding time is 30 to 50 minutes.
8. The preparation method according to claim 1, characterized in that: In step S1, the particle size after grinding is 10-15 μm; in step S2, the particle size of the powder after grinding is 40-70 μm.
9. A HfSiO4 bonding layer material, characterized in that: The method is prepared by any one of claims 1 to 8.
10. Use of the HfSiO4 bonding layer material according to claim 9 in preparing a HfSiO4 bonding layer.
Citation Information
Patent Citations
Hafnium silicate environment barrier coating for ceramic-based composite material matrix and preparation method thereof
CN111233446A
Method for preparing ZrO2 / ZrSiO4 multiphase ceramic through hot pressed sintering and application of ZrO2 / ZrSiO4 multiphase ceramic to radionuclide solidification
CN112142463A
Red pigment for zirconia ceramic, and preparation method and application thereof
CN112940535A
High-purity stable-phase gamma-yttrium pyrosilicate ceramic powder and preparation method thereof
CN116143516A
Low-temperature efficient preparation process of HfSiO4
CN116873944A