High-temperature piezoelectric ceramic for high-power scene and preparation method of high-temperature piezoelectric ceramic

By doping Mn elements in the Pb(Yb1/2Nb1/2)O3-PbZrO3-PbTiO3 system, the problem of high-power piezoelectric ceramic materials with both performance under high temperature and high pressure is solved, and high Curie temperature and high voltage electrical performance are achieved. Combined, suitable for high-power applications.

CN118930260AActive Publication Date: 2024-11-12XI AN JIAOTONG UNIV

Patent Information

Application Number
CN202410984288.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The problem of the high voltage electrical performance and high Curie temperature in the prior art is difficult to produce high-power piezoelectric ceramic materials.

Method used

By doping Mn elements in the Pb(Yb1/2Nb1/2)O3-PbZrO3-PbTiO3 system, using metal oxide MnO2 or composite oxide Pb(Mn1/3Nb2/3)O3, the composition of the material is adjusted to improve the mechanical quality factor and reduce losses to achieve excellent performance under high temperature and high pressure.

Benefits of technology

It achieves excellent comprehensive performance of high-power piezoelectric ceramic materials in high-temperature and high-voltage environments, and has both high Curie temperature and high-voltage electrical properties, and is suitable for the field of high-power transducers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930260A_ABST
    Figure CN118930260A_ABST
Patent Text Reader

Abstract

The invention discloses high-temperature piezoelectric ceramic for a high-power scene and a preparation method of the high-temperature piezoelectric ceramic, and belongs to the technical field of piezoelectric ceramic. The high-temperature piezoelectric ceramic is Mn element doped lead zirconate titanate based piezoelectric ceramic; the lead zirconate titanate base is a three-phase solid solution of Pb (Yb1 / 2Nb1 / 2) O3, PbZrO3 and PbTiO3; the doping mode of the Mn element is metal oxide MnO2 doping or composite oxide Pb (Mn1 / 3Nb2 / 3) O3 doping. According to the high-power high-temperature piezoelectric ceramic and the preparation method thereof, by controlling the components of the material, the process problem existing in material industrialization is solved, the problem that high piezoelectric performance, high Curie temperature and high mechanical quality factor are difficult to integrate is solved, and the high-power high-temperature piezoelectric ceramic with excellent comprehensive performance is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of piezoelectric ceramics, and specifically relates to a high-temperature piezoelectric ceramic for high-power scenarios and a preparation method thereof. Background Art

[0002] Piezoelectric ceramics are a type of functional material that realizes the mutual coupling and conversion (energy conversion) of mechanical energy and electrical energy. They are widely used in advanced manufacturing, electronic information, energy detection and national defense. For example, piezoelectric drives, ultrasonic motors, deep well acoustic wave detection, transducers and vibration sensors, etc. Piezoelectric ceramic materials are sensitive elements and core components of the entire system. In practical applications, some parameters that reflect the performance of materials are usually selected to evaluate the quality of materials. Common piezoelectric ceramic performance parameters mainly include piezoelectric constant, dielectric constant, mechanical quality factor Qm, dielectric loss tanδ, etc. High piezoelectric performance generally means that the main function of the system or device is better; and low loss means the performance stability of the device or system in long-term operation.

[0003] According to the performance characteristics, piezoelectric ceramics can generally be divided into two categories: "soft" and "hard". "Soft" piezoelectric ceramics have high piezoelectric, dielectric and electromechanical properties, and are mainly used in sensors, medical imaging, filters, etc. "Hard" piezoelectric ceramics have high mechanical quality factors and low dielectric losses. They are the core functional materials of high-power transmitting transducers, piezoelectric transformers, etc., and are widely used in sonar systems, ultrasonic detection, vibration control and other electromechanical conversion systems. In these applications, power-type piezoelectric modules need to generate large elastic strains under large electric power to exert their piezoelectric effect and then convert electromechanical energy. Continuous large-amplitude vibrations lead to large internal friction and dielectric losses and generate a lot of heat, which can easily cause stress damage, fatigue damage and performance deterioration. This requires high-power piezoelectric materials to have high mechanical quality factors Q on the basis of ensuring good "soft" performance. m And low dielectric loss tanδ, and has excellent and stable performance in alternating electric field and high temperature and high pressure environment.

[0004] Since the application environment of power ceramics is relatively harsh, high-power piezoelectric ceramics are required to have both high piezoelectric constant and high mechanical quality factor Q. m , low loss, high Curie temperature and other "soft and hard" properties. However, due to the influence of ferroelectric domains of piezoelectric ceramics, these properties are generally mutually restricted. For example, high "soft" performance often corresponds to low "hard" performance and low Curie temperature. The comprehensive requirements of these performance indicators make the preparation of high-power piezoelectric materials more difficult. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a high-temperature piezoelectric ceramic for high-power scenarios and a preparation method thereof. By controlling the composition of the material, the process problems existing in the industrialization of the material are solved, and the problem of difficulty in achieving both high voltage electrical performance and high Curie temperature and high mechanical quality factor is overcome, thereby obtaining a high-power high-temperature piezoelectric ceramic with excellent comprehensive performance.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides a high-temperature piezoelectric ceramic for high-power scenarios, wherein the high-temperature piezoelectric ceramic is a Mn-doped lead zirconate titanate-based piezoelectric ceramic; the lead zirconate titanate-based is Pb(Yb 1 / 2 Nb 1 / 2 ) a three-phase solid solution of PbO3, PbZrO3 and PbTiO3;

[0008] The doping method of the Mn element is metal oxide MnO2 doping or composite oxide Pb (Mn 1 / 3 Nb 2 / 3 )O3 doping.

[0009] In one embodiment, when the doping method of the Mn element is metal oxide MnO2 doping, the molecular formula of the Mn element doped lead zirconate titanate based piezoelectric ceramic is (1-xy)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zMnO2, wherein x ranges from 0.1 to 0.6, y ranges from 0.1 to 0.6, and z ranges from 0.01 to 0.1.

[0010] In one embodiment, the doping method of the Mn element is a composite oxide Pb (Mn 1 / 3 Nb 2 / 3 )O3 doped, the molecular formula of the Mn element doped lead zirconate titanate based piezoelectric ceramic is (1-xyz)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zPb(Mn 1 / 3 Nb 2 / 3 )O3, where x ranges from 0.1 to 0.6, y ranges from 0.1 to 0.6, and z ranges from 0.01 to 0.2.

[0011] The present invention also provides a method for preparing the high-temperature piezoelectric ceramic for high-power scenarios, comprising the following steps:

[0012] S1: preparing MnNb2O6 precursor powder or MnO2 and YbNbO4 precursor powder, mixing the ingredients according to the molecular formula of Mn element doped lead zirconate titanate based piezoelectric ceramics, and then ball milling, drying and sieving in sequence to obtain a raw material mixture;

[0013] S2: The raw material mixture is pre-calcined and then cooled to room temperature, and then ground to obtain pre-calcined powder;

[0014] S3: ball milling the pre-sintered powder, followed by drying, grinding and sieving to obtain ceramic powder;

[0015] S4: pressing the ceramic powder into a sheet to obtain a green piece, and then performing a pressureless closed sintering process on the green piece to obtain a fired piezoelectric ceramic;

[0016] S5: The fired piezoelectric ceramics are polished, silver-plated and polarized in sequence to obtain high-temperature piezoelectric ceramics for high-power scenarios.

[0017] In one embodiment, when the Mn element is derived from the MnNb2O6 precursor powder, the Mn element in the lead zirconate titanate-based piezoelectric ceramic is doped in the form of a composite oxide Pb(Mn 1 / 3 Nb 2 / 3 )O3 doping;

[0018] When the Mn element originates from MnO2, the doping mode of the Mn element in the Mn element-doped lead zirconate titanate-based piezoelectric ceramics is metal oxide MnO2 doping.

[0019] In one embodiment, in S1, the preparation process of the MnNb2O6 precursor powder is as follows:

[0020] According to the stoichiometric ratio of MnNb2O6, MnO2 and Nb2O5 are taken and mixed evenly, and then ball milling, drying, grinding, sieving are carried out in sequence, and then calcining is carried out at a temperature of 1000°C to 1200°C to obtain MnNb2O6 precursor powder.

[0021] In one embodiment, in S1, the preparation process of the YbNbO4 precursor powder is as follows:

[0022] Yb2O3 and Nb2O5 are taken according to the stoichiometric ratio of YbNbO4 and mixed evenly, and then ball milled, dried, ground, and sieved in sequence, and then calcined at a temperature of 1000°C to 1100°C to synthesize YbNbO4 precursor powder.

[0023] In one embodiment, in S2, the pre-burning process is as follows:

[0024] The temperature is raised to 750°C-850°C at a heating rate of 2-10°C / min and pre-fired for 2-5h.

[0025] In one embodiment, in S4, the process of the pressureless closed sintering treatment is as follows:

[0026] The blank is buried in homogeneous ceramic powder and placed on a zirconia flat plate. The zirconia flat plate is placed in an alumina closed sagger and heated to 1100-1300°C at a heating rate of 2-5°C / min. It is sintered for 3-5h and then naturally cooled to room temperature in the furnace.

[0027] In one embodiment, in S5, the polishing process is as follows:

[0028] The upper and lower surfaces of the fired piezoelectric ceramics were polished with 600-2000 mesh sandpaper, and then polished with metallographic sandpaper to a thickness of 0.8-1.2 mm, and then ultrasonically cleaned with deionized water and ethanol in turn, and then dried;

[0029] The silver plating process is as follows:

[0030] The silver paste is evenly coated on the upper and lower surfaces of the polished fired piezoelectric ceramic, and then placed in a resistance furnace, kept at a temperature of 500°C to 850°C for 5min to 60min, and naturally cooled to room temperature along with the furnace;

[0031] The polarization process is as follows:

[0032] The silver-plated fired piezoelectric ceramic is placed in silicone oil and polarized along the thickness direction using a direct current electric field or an alternating current electric field; the polarization temperature is 90°C to 150°C, the polarization voltage is 10kV / cm to 50kV / cm, and the polarization voltage holding time is 10 to 60 minutes.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The present invention provides a high-temperature piezoelectric ceramic for high-power scenarios, wherein the high-temperature piezoelectric ceramic is a lead zirconate titanate-based piezoelectric ceramic doped with Mn element; wherein the doping method of Mn element is metal oxide MnO2 doping or composite oxide Pb (Mn 1 / 3Nb 2 / 3 )O3 doping, the design idea is to hard dope the PYN-PZT high temperature piezoelectric ceramics to increase the mechanical quality factor and reduce the loss. 2+ / 3+ Replaced Ti 4+ / Zr 4+, excess negative charges appear in the lattice. In order to maintain electrical neutrality, oxygen vacancies are generated, and oxygen vacancies cause cell contraction, resulting in a "pinning effect" that makes it difficult for domain walls to move, thereby reducing the loss caused by domain wall movement and increasing the mechanical quality factor. At the same time, the introduction of Mn elements will reduce piezoelectric properties, but because the PYN-PZT system has the characteristics of high Curie temperature and high piezoelectric properties, the Mn-doped lead zirconate titanate-based piezoelectric ceramics can improve the mechanical quality factor while still maintaining a high Curie temperature and piezoelectric properties.

[0035] Furthermore, metal oxide MnO2 and composite oxide Pb(Mn 1 / 3 Nb 2 / 3 )O3-doped PYN-PZT-based piezoelectric ceramics have high high-power performance and Curie temperature, and their Curie temperature is higher than 350℃. 33 Higher than 250pC / N. Coercive field E of PYN-PZT based piezoelectric ceramics doped with metal oxide MnO2 C Up to 25kV / cm, internal bias field E i Up to 5kV / cm, Q m The vibration speed can reach 1800, and the vibration speed can reach 0.8m / s. The loss change rate is about 80% under the strong alternating electric field. 1 / 3 Nb 2 / 3 ) Coercive Field E of O3-doped PYN-PZT-based Piezoelectric Ceramics C Up to 26kV / cm, internal bias field E i Up to 8.5kV / cm, Q m The vibration speed can reach 3000, the vibration speed can reach 1m / s, and the loss change rate under strong alternating electric field is only 30%. The above shows that Mn-doped PYN-PZT high-temperature piezoelectric ceramics can be used in high-power applications under strong field or strong drive. In addition, the above content further shows that the hard composite oxide Pb (Mn 1 / 3 Nb 2 / 3 )O3 doping has better high-power performance than metal oxide MnO2 doping. Therefore, this study is helpful to the design of high-power piezoelectric ceramics to a certain extent.

[0036] The present invention also provides a method for preparing high-temperature piezoelectric ceramics for high-power scenarios, wherein the preparation method obtains fired piezoelectric ceramics by preparing ceramic powder and performing pressureless and closed sintering on the ceramic powder. The use of pressureless and closed sintering means that no external pressure is applied to the blank during the sintering process, which helps to reduce the deformation or rupture of the ceramic structure caused by pressure. The airtightness ensures the stability and consistency of the sintering environment and reduces the interference of external factors (such as oxygen, moisture, etc.) on the sintering process. Conventional sintering treatments may include applying external pressure or using an open sintering environment, which may lead to unevenness of the ceramic structure or contamination by external factors. Pressureless and closed sintering can more accurately control the sintering process by avoiding the above potential problems, thereby obtaining piezoelectric ceramics with a pure perovskite crystal structure, a dense microstructure, and uniform grain size, which is beneficial to improving the comprehensive performance of high-power piezoelectric ceramics. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 A cross-sectional morphology image of a scanning electron microscope (SEM) image of a PMnN-doped PYN-PZT piezoelectric ceramic prepared in Example 8 of the present invention;

[0038] Figure 2 The dielectric constant of MnO2 and PMnN doped PYN-PZT prepared in Examples 1, 2, 4 and 5 of the present invention varies with temperature;

[0039] Figure 3 The hysteresis loop diagram of the PYN-PZT piezoelectric ceramics prepared in Examples 3 and 6 of the present invention;

[0040] Figure 4 The impedance diagram and phase angle diagram of the PMnN-doped PYN-PZT ceramic prepared in Example 6;

[0041] Figure 5 A schematic diagram of the vibration velocity of the PMnN-doped PYN-PZT ceramic prepared in Example 5;

[0042] Figure 6 Schematic diagram of the loss of MnO2 and PMnN doped PYN-PZT ceramics prepared in Examples 2 and 5 under a strong AC electric field;

[0043] Figure 7 XRD patterns of PYN-PZT, MnO2-doped PYN-PZT and PMnN-doped PYN-PZT piezoelectric ceramics. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0045] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0046] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0047] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0048] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0049] The present invention provides a high-temperature piezoelectric ceramic for high-power scenarios and a preparation method thereof. The present invention obtains high-temperature piezoelectric ceramics for high-power scenarios with excellent comprehensive performance through material composition and controlled ceramic sintering process, solves the process problems existing in material industrialization, and overcomes the problem that it is difficult to have both high voltage electrical performance and high Curie temperature and high mechanical quality factor.

[0050] In the study of piezoelectric materials, a common method to improve high-power performance is to use hard doping (such as Cr 3+ , Fe 2 / 3+ etc.), and the present invention designs the composition of piezoelectric ceramics to obtain Pb(Yb 1 / 2 Nb 1 / 2 )O3-PbZrO3-PbTiO3 system, by doping with metal oxide MnO2 and composite oxide Pb(Mn 1 / 3 Nb 2 / 3)O3(PMnN) doping methods introduce Mn elements. Both doping methods can obtain high-power piezoelectric ceramics with excellent comprehensive performance. They have high Curie temperature, high softness and high hardness, which makes them have considerable application prospects in power devices. In addition, the research results of this project show that the composite oxide Pb(Mn 1 / 3 Nb 2 / 3 )O3(PMnN) doping has better high-power performance than metal oxide MnO2 doping. Therefore, this study is helpful to the design of high-power piezoelectric ceramics to a certain extent.

[0051] On the one hand, the present invention provides a high-temperature piezoelectric ceramic for high-power scenarios, wherein the high-temperature piezoelectric ceramic is a Mn-doped lead zirconate titanate-based piezoelectric ceramic (Pb(Yb 1 / 2 Nb 1 / 2 )O3-PbZrO3-PbTiO3 ceramic), the lead zirconate titanate base is Pb(Yb 1 / 2Nb 1 / 2 )O3, PbZrO3 and PbTiO3 three-phase solid solution, the Mn element is doped in the form of metal oxide MnO2 doping or composite oxide Pb(Mn 1 / 3 Nb 2 / 3 )O3 doped, the piezoelectric ceramic has a perovskite structure.

[0052] When the Mn element is doped with metal oxide MnO2, the molecular formula of the Mn element doped lead zirconate titanate based piezoelectric ceramic is (1-xy)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zMnO2 (x ranges from 0.1 to 0.6, y ranges from 0.1 to 0.6, and z ranges from 0.01 to 0.1).

[0053] The doping method of Mn element is composite oxide Pb(Mn 1 / 3 Nb 2 / 3 )O3 doped, the molecular formula of Mn-doped lead zirconate titanate-based piezoelectric ceramics is (1-xyz)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zPb(Mn 1 / 3 Nb 2 / 3 )O3 (x value range is 0.1-0.6, y value range is 0.1-0.6, z value range is 0.01-0.2).

[0054] The Q of the MnO2-doped PYN-PZT piezoelectric ceramics m can reach 1800, and the vibration speed can reach 0.8m / s. 1 / 3Nb 2 / 3 )Q of O3-doped PYN-PZT piezoelectric ceramics m It can reach 3000, and the vibration speed can reach 1m / s, which is suitable for the field of high-power transducers.

[0055] The present invention also provides a method for preparing high-temperature piezoelectric ceramics for high-power scenarios, comprising the following steps:

[0056] S1: preparing MnNb2O6 precursor powder or MnO2 and YbNbO4 precursor powder, mixing the ingredients according to the molecular formula of Mn element doped lead zirconate titanate based piezoelectric ceramics, and then ball milling, drying and sieving in sequence to obtain a raw material mixture; specifically, when the Mn element is derived from the MnNb2O6 precursor powder, the Mn element in the Mn element doped lead zirconate titanate based piezoelectric ceramics is doped in the form of a composite oxide Pb (Mn 1 / 3 Nb 2 / 3 )O3 doping; when the Mn element is derived from MnO2, the doping method of the Mn element in the lead zirconate titanate-based piezoelectric ceramic is metal oxide MnO2 doping;

[0057] S2: The raw material mixture is pre-calcined and then cooled to room temperature, and then ground to obtain pre-calcined powder;

[0058] S3: ball milling the pre-sintered powder, followed by drying, grinding and sieving to obtain ceramic powder;

[0059] S4: pressing the ceramic powder into a sheet to obtain a green piece, and then performing a pressureless closed sintering process on the green piece to obtain a fired piezoelectric ceramic;

[0060] S5: The fired piezoelectric ceramics are polished, silver-plated and polarized in sequence to obtain high-temperature piezoelectric ceramics for high-power scenarios.

[0061] In a specific embodiment, in S1, the preparation process of the MnNb2O6 precursor powder is as follows: MnO2 and Nb2O5 are taken according to the stoichiometric ratio of MnNb2O6 and mixed evenly, and then ball milled, dried, ground, and sieved in sequence, and then calcined at a temperature of 1000°C to 1200°C to obtain the MnNb2O6 precursor powder.

[0062] In a specific implementation, in S1, the preparation process of the YbNbO4 precursor powder is as follows: Yb2O3 and Nb2O5 are taken according to the stoichiometric ratio of YbNbO4 and mixed evenly, and then ball milled, dried, ground, and sieved in sequence, and then calcined at a temperature of 1000°C to 1100°C to synthesize the YbNbO4 precursor powder.

[0063] In a specific implementation manner, in S2, the pre-firing process is as follows: heating to 750°C-850°C at a heating rate of 2-10°C / min and pre-firing for 2-5h.

[0064] In a specific implementation, in S4, the process of pressureless closed sintering treatment is as follows: bury the blank in homogeneous ceramic powder, place it on a zirconia plate, place the zirconia plate in an alumina closed sagger, heat it to 1100-1300°C at a heating rate of 2-5°C / min, sinter it for 3-5h, and then naturally cool it to room temperature with the furnace. Pressureless closed sintering treatment improves the stability and controllability of the sintering process, helps to obtain a more uniform ceramic structure, reduces the interference of external factors on the sintering process, reduces the risk of ceramic contamination, and helps to improve the quality and performance of fired piezoelectric ceramics, especially for high-temperature applications in high-power scenarios.

[0065] In a specific implementation, in S5, the polishing process is as follows: use 600-2000 mesh sandpaper to grind the upper and lower surfaces of the fired piezoelectric ceramic, then use metallographic sandpaper to polish to a thickness of 0.8-1.2 mm, then use deionized water and ethanol ultrasonic cleaning in turn, and then dry.

[0066] In a specific implementation, in S5, the silver plating process is as follows: silver paste is evenly coated on the upper and lower surfaces of the polished and fired piezoelectric ceramic, and then placed in a resistance furnace at a temperature of 500°C to 850°C for 5min to 60min, and naturally cooled to room temperature with the furnace.

[0067] In a specific implementation, in S5, the polarization process is as follows: the fired piezoelectric ceramic after silver plating is placed in silicone oil, and polarized along the thickness direction using a DC electric field or an AC electric field; the polarization temperature is 90°C to 150°C, the polarization voltage is 10kV / cm to 50kV / cm, and the polarization voltage is maintained for 10 to 60 minutes.

[0068] More specifically, a method for preparing high-temperature piezoelectric ceramics for high-power scenarios is provided, and the specific steps are as follows:

[0069] Step 1: Preparation of ceramic powder:

[0070] When metal oxide MnO2 is used to dope lead zirconate titanate based piezoelectric ceramics, the molecular formula of the ceramic powder is (1-xy)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zMnO2, the method for preparing the above ceramic powder is as follows:

[0071] (1) Preparation of YbNbO4 precursor powder

[0072] According to the stoichiometric ratio of YbNbO4, Yb2O3 and Nb2O5 are weighed as raw materials respectively, all the weighed raw materials are mixed evenly and put into a nylon jar, zirconium oxide balls are used as grinding balls and anhydrous ethanol is used as ball milling medium, and the mixture is fully mixed and ball milled at 150-300 rpm for 18-72 hours in a ball mill, and the zirconium balls are separated, and the raw material mixture is dried at 80°C-100°C for 12-24 hours, ground with a mortar, and passed through a 80-200 mesh sieve; the sieved powder is placed in an alumina crucible, covered, and calcined at 1000°C-1100°C for 5-10 hours to synthesize a YbNbO4 precursor powder;

[0073] (2) Ingredients

[0074] According to (1-xy)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zMnO2 stoichiometric ratio (x ranges from 0.1-0.6, y ranges from 0.1-0.6, z ranges from 0.01-0.1) is used for mixing. For example, 0.2Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.3PbZrO3-0.5PbTiO3+0.05MnO2, respectively weighing 67.0748g of PbO with a purity of 99.9%, 9.9157g of YbNbO4, 11.1091g of ZrO2 with a purity of 99.9%, 12.0004g of TiO2 with a purity of 99.9% and 0.3955g of MnO2 with a purity of 99% as raw materials, mixing all the weighed raw materials uniformly and putting them into a nylon jar, using zirconium balls as grinding balls and anhydrous ethanol as ball milling media, fully mixing and ball milling for 18 to 72 hours, separating the zirconium balls, drying the raw material mixture at 80 to 100° C. for 12 to 24 hours, grinding with a mortar, and passing through a 80 to 200 mesh sieve to obtain a raw material mixture;

[0075] (3) Pre-burning

[0076] The sieved raw material mixture in step (2) is placed in an alumina crucible, compacted with an agate rod, covered, placed in a resistance furnace, and pre-fired at 750° C. to 850° C. for 2 to 5 hours at a heating rate of 2 to 10° C. / min, cooled naturally to room temperature, removed from the furnace, and ground with a mortar to obtain pre-fired powder;

[0077] (4) Secondary ball milling

[0078] The calcined powder was put into a nylon jar, and zirconium balls were used as grinding balls and anhydrous ethanol was used as the grinding medium. The mixture was fully mixed and ball-milled for 18 to 72 hours using a ball mill at 150 to 300 rpm. The zirconium balls were separated, and the calcined powder was dried at 80 to 100°C for 12 to 48 hours, ground with a mortar, and passed through a 80 to 200 mesh sieve to obtain (1-xy)Pb(Yb1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zMnO2 ceramic powder.

[0079] When the composite oxide Pb(Mn 1 / 3 Nb 2 / 3 )O3 doped lead zirconate titanate based piezoelectric ceramics, the molecular formula of the ceramic powder is (1-xyz)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zPb(Mn 1 / 3 Nb 2 / 3 )O3, the method for preparing the aforementioned ceramic powder is as follows:

[0080] (1) Preparation of YbNbO4 and MnNb2O6 precursor powders

[0081] YbNbO4 precursor powder: according to the stoichiometric ratio of YbNbO4, Yb2O3 and Nb2O5 are weighed as raw materials respectively, all the weighed raw materials are mixed evenly and put into a nylon jar, zirconium oxide balls are used as grinding balls and anhydrous ethanol is used as ball milling medium, and the mixture is fully mixed and ball milled at 150-300 rpm for 18-24 hours in a ball mill, and the zirconium balls are separated. The raw material mixture is dried at 80°C to 100°C for 12-48 hours, ground with a mortar, and passed through a 80-200 mesh sieve; the sieved powder is placed in an alumina crucible, covered, and calcined at 1000°C to 1100°C for 5-10 hours to synthesize the YbNbO4 precursor powder;

[0082] MnNb2O6 precursor powder: according to the stoichiometric ratio of MnNb2O6, MnO2 and Nb2O5 are weighed as raw materials respectively, all the weighed raw materials are mixed evenly and put into a nylon jar, zirconium oxide balls are used as grinding balls and anhydrous ethanol is used as ball milling medium, and the mixture is fully mixed and ball milled at 150-300 rpm for 18-72 hours in a ball mill, and the zirconium balls are separated. The raw material mixture is dried at 80°C-100°C for 12-48 hours, ground with a mortar, and passed through a 80-200 mesh sieve; the sieved powder is placed in an alumina crucible, covered, and calcined at 1000°C-1200°C for 5-10 hours to synthesize the MnNb2O6 precursor powder;

[0083] (2) Ingredients

[0084] According to (1-xyz)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zPb(Mn 1 / 3 Nb 2 / 3)O3 stoichiometric ratio (x ranges from 0.1-0.6, y ranges from 0.1-0.6, z ranges from 0.01-0.2) is used for mixing. For example, 0.05Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.3PbZrO3-0.5PbTiO3+0.15Pb(Mn 1 / 3 Nb 2 / 3 )O3, weigh 68.7063g of PbO with a purity of 99.9%, 2.5392g of YbNbO4, 11.3793g of ZrO2 with a purity of 99.9%, 12.2923g of TiO2 with a purity of 99.9% and 5.1830g of MnNb2O6 as raw materials respectively, mix all the weighed raw materials evenly and put them into a nylon jar, use zirconium balls as grinding balls and anhydrous ethanol as ball milling media, mix and mill them thoroughly for 18 to 72 hours, separate the zirconium balls, dry the raw material mixture at 80 to 100° C. for 12 to 48 hours, grind it with a mortar, and pass it through a 80 to 200 mesh sieve to obtain a raw material mixture;

[0085] (3) Pre-burning

[0086] The sieved raw material mixture in step (2) is placed in an alumina crucible, compacted with an agate rod, covered, placed in a resistance furnace, and pre-fired at 700°C to 950°C at a heating rate of 2 to 10°C / min for 2 to 8 hours, naturally cooled to room temperature, removed from the furnace, and ground with a mortar to obtain pre-fired powder;

[0087] (4) Secondary ball milling

[0088] The calcined powder was put into a nylon jar, and zirconium balls were used as grinding balls and anhydrous ethanol was used as the grinding medium. The mixture was fully mixed and ball-milled in a ball mill at 150-300 rpm for 18-72 hours. The zirconium balls were separated, and the calcined powder was dried at 80-100°C for 12-48 hours, ground in a mortar, and passed through a 80-200 mesh sieve to obtain (1-xyz)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zPb(Mn 1 / 3 Nb 2 / 3 )O3 ceramic powder.

[0089] Step 2: Prepare PYN-PZT-based high-temperature piezoelectric ceramics for high-power scenarios:

[0090] (1) Tableting

[0091] The two ceramic powders after being sieved through 80-200 meshes are respectively pressed into cylindrical blanks by a powder tablet press, and then cold isostatically pressed at a pressure of 200-300 MPa for 15-20 minutes;

[0092] (2) Pressureless sealed sintering

[0093] The two cylindrical blanks with different compositions are respectively buried in their respective homogeneous powders and placed on a zirconia flat plate. The zirconia flat plate is placed in an alumina closed sagger and heated to 1100-1300°C at a heating rate of 2-5°C / min. The blanks are sintered for 3-5 hours and naturally cooled to room temperature in the furnace to obtain fired piezoelectric ceramics.

[0094] (3) Polishing

[0095] The upper and lower surfaces of the two piezoelectric ceramics sintered in step (2) were polished with 600-2000 mesh sandpaper, and then polished with metallographic sandpaper to a thickness of 0.8-1.2 mm, and then ultrasonically cleaned with deionized water and ethanol, respectively, and dried;

[0096] (4) Silver-plated electrode

[0097] The silver paste is evenly coated on the two surfaces of the ceramic after polishing, and the ceramic is placed in a resistance furnace. The temperature is kept at 500°C to 850°C for 5 minutes to 60 minutes, and the ceramic is naturally cooled to room temperature along with the furnace to obtain a piezoelectric ceramic plated with silver electrodes.

[0098] (5) Polarization

[0099] The two piezoelectric ceramics after silver plating in step (4) are placed in silicone oil and polarized along the thickness direction using a DC electric field or an AC electric field. The polarization temperature is 90°C to 150°C, the polarization voltage is 10 kV / cm to 50 kV / cm, and the polarization voltage is maintained for 10 to 60 minutes to obtain chemical formulas of (1-xy)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zMnO2 and (1-xyz)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zPb(Mn 1 / 3 Nb 2 / 3 )O3 piezoelectric ceramics.

[0100] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0101] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples that do not specify specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples, unless otherwise specified, are conventional commercially available products, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0102] Example

[0103] The general formula of the high-temperature piezoelectric ceramic for high-power scenarios provided by the embodiment of the present invention is:

[0104] When the Mn element originates from the metal oxide MnO2, the metal oxide MnO2 is doped with Pb(Yb 1 / 2 Nb 1 / 2 )O3-PbZrO3-PbTiO3:

[0105] The molecular formula of Example 1 is 0.2Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.2PbZrO3-0.6PbTiO3+0.01MnO2;

[0106] The molecular formula of Example 2 is 0.1Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.6PbZrO3-0.3PbTiO3+0.03MnO2;

[0107] The molecular formula of Example 3 is 0.45Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.45PbZrO3-0.1PbTiO3+0.05MnO2;

[0108] The molecular formula of Example 4 is 0.4Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.1PbZrO3-0.5PbTiO3+0.1MnO2;

[0109] When the Mn element is derived from the MnNb2O6 precursor powder, the composite oxide Pb(Mn 1 / 3 Nb 2 / 3 )O3 doped Pb(Yb 1 / 2 Nb 1 / 2 )O3-PbZrO3-PbTiO3:

[0110] The molecular formula of Example 5 is 0.19Pb(Yb 1 / 2 Nb 1 / 2)O3-0.2PbZrO3-0.6PbTiO3+0.01Pb(Mn 1 / 3Nb 2 / 3 )O3;

[0111] The molecular formula of Example 6 is 0.01Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.6PbZrO3-0.3PbTiO3+0.09Pb(Mn 1 / 3Nb 2 / 3 )O3;

[0112] The molecular formula of Example 7 is 0.3Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.45PbZrO3-0.1PbTiO3+0.15Pb(Mn 1 / 3Nb 2 / 3 )O3;

[0113] The molecular formula of Example 8 is 0.2Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.1PbZrO3-0.5PbTiO3+0.2Pb(Mn 1 / 3 Nb 2 / 3 )O3.

[0114] Example 1

[0115] Preparation of metal oxide MnO2 doped PYN-PZT ceramics:

[0116] (1) Preparation of YbNbO4 precursor powder

[0117] According to the stoichiometric ratio of YbNbO4, 59.7804g of Yb2O3 with a purity of 99.9% and 40.3197g of Nb2O5 with a purity of 99.9% were weighed as raw materials, all the weighed raw materials were mixed evenly and put into a nylon jar, zirconium oxide balls were used as grinding balls, anhydrous ethanol was used as ball milling medium, the mass ratio of anhydrous ethanol to the raw material mixture was 1:1.2, and the mixture was ball milled at 250 rpm for 48 hours, the zirconium balls were separated, and the raw material mixture was placed in a drying oven at 80°C for 24 hours, ground with a mortar for 30 minutes, and passed through a 200-mesh sieve; the sieved powder was placed in an alumina crucible, covered, and calcined at 1000°C for 10 hours to synthesize YbNbO4 precursor powder;

[0118] (2) Ingredients

[0119] For 0.2Pb(Yb 1 / 2 Nb 1 / 2)O3-0.2PbZrO3-0.6PbTiO3+0.01MnO2 samples, according to 0.2Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.2PbZrO3-0.6PbTiO3+0.01MnO2 chemical measurement, weigh 7.9594g PbO6 with a purity of 99.9%, 10.0465g YbNbO4, 7.5037g ZrO2 with a purity of 99.9%, 14.5905g TiO2 with a purity of 99.9% and 0.2671g MnO2 with a purity of 99% as raw materials; put the raw material mixture into a nylon jar, use zirconium balls as grinding balls and anhydrous ethanol as ball milling media, the mass ratio of anhydrous ethanol to the raw material mixture is 1:1.2, use a ball mill at 250 rpm for 48 hours, separate the zirconium balls, place the raw material mixture in a drying oven at 80°C for 14 hours, grind it with a mortar for 30 minutes, and pass it through a 80-mesh sieve.

[0120] (3) Pre-burning

[0121] The raw material mixture after passing through an 80-mesh sieve in step (2) was placed in an alumina crucible and compacted with an agate rod to a compacted density of 1.5 g / cm 3 , cover, place in a resistance furnace, heat to 850℃ at a heating rate of 3℃ / min, pre-fire for 5 hours, cool naturally to room temperature, take out of the furnace, grind in a mortar for 30 minutes, and obtain pre-fired powder.

[0122] (4) Secondary ball milling

[0123] The calcined powder was put into a nylon jar, and zirconium balls were used as grinding balls and anhydrous ethanol was used as the grinding medium. The mass ratio of anhydrous ethanol to calcined powder was 1:1.2. The calcined powder was milled at 250 rpm for 72 hours. The zirconium balls were separated and the calcined powder was dried in a drying oven at 80°C for 15 hours. The calcined powder was ground with a mortar for 10 minutes and passed through a 200-mesh sieve to obtain 0.2Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.2PbZrO3-0.6PbTiO3+0.01MnO2 powder.

[0124] (5) Tablet pressing

[0125] The ceramic powder after passing through a 200-mesh sieve was pressed into a cylindrical blank using a powder tablet press, and then cold isostatically pressed at a pressure of 300 MPa for 20 minutes;

[0126] (6) Pressureless sealed sintering

[0127] The cylindrical blank is buried in the respective homogeneous powders and placed on a zirconia flat plate. The zirconia flat plate is placed in an alumina closed sagger and heated to 1300°C at a heating rate of 5°C / min. The sintering is performed for 5 hours and the sintered piezoelectric ceramic is obtained after being naturally cooled to room temperature in the furnace.

[0128] (7) Polishing

[0129] The upper and lower surfaces of the piezoelectric ceramic sintered in step (6) were polished with 2000-mesh sandpaper, and then polished with metallographic sandpaper to a thickness of 1.2 mm, and then ultrasonically cleaned with deionized water and ethanol, respectively, and dried;

[0130] (8) Silver-plated electrode

[0131] The silver paste is evenly coated on the two surfaces of the ceramic after polishing, and the ceramic is placed in a resistance furnace. The temperature is kept at 850°C for 60 minutes, and the ceramic is naturally cooled to room temperature along with the furnace to obtain a piezoelectric ceramic plated with silver electrodes.

[0132] (9) Polarization

[0133] The silver-plated piezoelectric ceramic in step (8) is placed in silicone oil and polarized along the thickness direction using a DC electric field or an AC electric field. The polarization temperature is 150° C., the polarization voltage is 50 kV / cm, and the polarization voltage is maintained for 60 minutes to obtain a chemical formula of 0.2Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.2PbZrO3-0.6PbTiO3+0.01MnO2 piezoelectric ceramics.

[0134] Example 2

[0135] Preparation of ceramic powder: For 0.1Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.6PbZrO3-0.3PbTiO3+0.03MnO2, according to 0.1Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.6PbZrO3-0.3PbTiO3+0.03MnO2, 99.9% PbO 66.1816g, YbNbO4 4.8918g, 99.9% pure ZrO2 21.9223g, 99.9% pure TiO2 7.1044g and 99% pure MnO2 0.7804g were weighed as raw materials and mixed evenly to prepare 0.1Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.6PbZrO3-0.3PbTiO3+0.03MnO2 piezoelectric ceramic powder.

[0136] Tabletting: The ceramic powder after passing through an 80-mesh sieve is pressed into a cylindrical blank using a powder tablet press, and then cold isostatically pressed at a pressure of 200 MPa for 15 minutes.

[0137] Pressureless closed sintering: bury the cylindrical blank in homogeneous powder, place it on a zirconia plate, place the zirconia plate in an alumina closed sagger, heat it to 1100℃ at a heating rate of 2℃ / min, sinter for 3 hours, and cool it naturally to room temperature in the furnace to obtain the fired piezoelectric ceramics.

[0138] Polishing: The upper and lower surfaces of the sintered piezoelectric ceramics were polished with 600-grit sandpaper, and then polished with metallographic sandpaper to a thickness of 0.8 mm, and then ultrasonically cleaned with deionized water and ethanol, respectively, and dried.

[0139] Silver-plated electrode: Evenly coat the silver paste on the two polished surfaces of the ceramic, place it in a resistance furnace, keep it warm at 500°C for 5 minutes, and naturally cool it to room temperature with the furnace to obtain piezoelectric ceramics plated with silver electrodes.

[0140] Polarization: Place the silver-plated piezoelectric ceramic in silicone oil and polarize it along the thickness direction using a DC electric field or an AC electric field. The polarization temperature is 90°C, the polarization voltage is 10 kV / cm, and the polarization voltage is maintained for 10 minutes. The chemical formula is 0.1Pb(Yb 1 / 2 Nb 1 / 2 )Piezoelectric ceramics of O3-0.6PbZrO3-0.3PbTiO3+0.03MnO2.

[0141] The other steps and process parameters are the same as those in Example 1.

[0142] Example 3

[0143] Preparation of ceramic powder: For 0.45Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.45PbZrO3-0.1PbTiO3+0.05MnO2, according to 0.45Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.45PbZrO3-0.1PbTiO3+0.05MnO2 stoichiometry, weigh 61.9111g of PbO with a purity of 99.9%, 20.5929 of YbNbO4, and 99.9% of ZrO2

[0144] 15.3808g, 99.9% pure TiO2 2.2153g and 99% pure MnO2 1.2167g were mixed as raw materials to prepare 0.45Pb(Yb 1 / 2 Nb 1 / 2)O3-0.45PbZrO3-0.1PbTiO3+0.05MnO2 piezoelectric ceramic powder.

[0145] Tabletting: The ceramic powder after passing through a 150-mesh sieve is pressed into a cylindrical blank using a powder tablet press, and then cold isostatically pressed at a pressure of 300 MPa for 20 minutes.

[0146] Pressureless closed sintering: bury the cylindrical blank in homogeneous powder, place it on a zirconia plate, place the zirconia plate in an alumina closed sagger, heat it to 1300℃ at a heating rate of 2℃ / min, sinter it for 5 hours, and cool it naturally to room temperature in the furnace to obtain the fired piezoelectric ceramics.

[0147] Polishing: The upper and lower surfaces of the sintered piezoelectric ceramics were polished with 2000-grit sandpaper, and then polished with metallographic sandpaper to a thickness of 1 mm, and then ultrasonically cleaned with deionized water and ethanol, respectively, and dried.

[0148] Silver-plated electrode: Evenly coat the silver paste on the two polished surfaces of the ceramic, place it in a resistance furnace, keep it warm for 60 minutes at 650°C, and naturally cool it to room temperature with the furnace to obtain piezoelectric ceramics plated with silver electrodes.

[0149] Polarization: Place the silver-plated piezoelectric ceramic in silicone oil and polarize it along the thickness direction using a DC electric field or an AC electric field. The polarization temperature is 150°C, the polarization voltage is 50 kV / cm, and the polarization voltage is maintained for 60 minutes. The chemical formula is 0.45Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.45PbZrO3-0.1PbTiO3+0.05MnO2 piezoelectric ceramics.

[0150] The other steps and process parameters are the same as those in Example 1.

[0151] Example 4

[0152] Preparation of ceramic powder: For 0.4Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.1PbZrO3-0.5PbTiO3+0.1MnO2, according to 0.4Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.1PbZrO3-0.5PbTiO3+0.1MnO2 stoichiometry, weigh 65.4342g of PbO with a purity of 99.9%, 19.3464g of YbNbO4, and 99.9% pure ZrO2

[0153] 3.6125g, 99.9% pure TiO2 11.7069g and 99% pure MnO2 2.5719g were mixed as raw materials to prepare 0.4Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.1PbZrO3-0.5PbTiO3+0.1MnO2 piezoelectric ceramic powder.

[0154] The other steps and process parameters are the same as those in Example 1.

[0155] Example 5

[0156] Preparation of Pb(Mn 1 / 3 Nb 2 / 3 )O3 doped PYN-PZT ceramics:

[0157] (1) Preparation of YbNbO4 and MnNb2O6 precursor powders

[0158] The preparation method of YbNbO4 precursor powder is as shown in (1) in the above-mentioned Example 1.

[0159] MnNb2O6 precursor powder: according to the stoichiometric ratio of MnNb2O6, 24.8953g of MnO2 with a purity of 99% and 75.4291g of Nb2O5 with a purity of 99.9% were weighed as raw materials, all the weighed raw materials were mixed evenly and put into a nylon jar, and zirconia balls were used as grinding balls and anhydrous ethanol was used as ball milling media, and the mixture was fully mixed and ball milled at 300 rpm for 24 hours in a ball mill, and the zirconium balls were separated. The raw material mixture was dried at 100°C for 24 hours, ground with a mortar, and passed through an 80-mesh sieve; the sieved powder was placed in an alumina crucible, covered, and calcined at 1200°C for 8 hours to synthesize the MnNb2O6 precursor powder;

[0160] (2) Ingredients

[0161] For 0.19Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.2PbZrO3-0.6PbTiO3+0.01Pb(Mn 1 / 3 Nb 2 / 3 )O3 samples, according to 0.19Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.2PbZrO3-0.6PbTiO3+0.01Pb(Mn 1 / 3 Nb 2 / 3)O3 stoichiometrically, 68.0685g of PbO with a purity of 99.9%, 9.5595g of YbNbO4, 7.5158g of ZrO2 with a purity of 99.9%, 14.6139g of TiO2 with a purity of 99.9% and 0.3423g of MnNb2O6 were weighed as raw materials respectively; the raw material mixture was put into a nylon jar, zirconium balls were used as grinding balls, anhydrous ethanol was used as ball milling medium, the mass ratio of anhydrous ethanol to the raw material mixture was 1:1.2, and ball milling was carried out at 250 rpm for 48 hours, the zirconium balls were separated, and the raw material mixture was placed in a drying oven and dried at 80°C for 24 hours, ground with a mortar for 30 minutes, and passed through a 200-mesh sieve.

[0162] (3) Pre-burning

[0163] The sieved raw material mixture in step (2) is placed in an alumina crucible, compacted with an agate rod, covered, placed in a resistance furnace, and pre-fired to 950° C. at a heating rate of 2° C. / min for 5 hours, naturally cooled to room temperature, removed from the furnace, and ground with a mortar to obtain pre-fired powder;

[0164] (4) Secondary ball milling

[0165] The calcined powder was put into a nylon jar, and zirconium balls were used as grinding balls and anhydrous ethanol was used as the grinding medium. The mixture was fully mixed and ball-milled at 150-300 rpm for 72 hours. The zirconium balls were separated, and the calcined powder was dried at 100°C for 24 hours. The calcined powder was ground with a mortar and passed through a 200-mesh sieve to obtain

[0166] 0.19Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.2PbZrO3-0.6PbTiO3+0.01Pb(Mn 1 / 3 Nb 2 / 3 )O3 powder.

[0167] (5) Tablet pressing

[0168] The ceramic powder after passing through a 200-mesh sieve was pressed into a cylindrical blank using a powder tablet press, and then cold isostatically pressed at a pressure of 300 MPa for 20 minutes;

[0169] (6) Pressureless sealed sintering

[0170] The cylindrical blank is buried in the respective homogeneous powders and placed on a zirconia flat plate. The zirconia flat plate is placed in an alumina closed sagger and heated to 1300°C at a heating rate of 5°C / min. The sintering is performed for 5 hours and the sintered piezoelectric ceramic is obtained after being naturally cooled to room temperature in the furnace.

[0171] (7) Polishing

[0172] The upper and lower surfaces of the piezoelectric ceramic sintered in step (6) were polished with 2000-mesh sandpaper, and then polished with metallographic sandpaper to a thickness of 1.2 mm, and then ultrasonically cleaned with deionized water and ethanol, respectively, and dried;

[0173] (8) Silver-plated electrode

[0174] The silver paste is evenly coated on the two surfaces of the ceramic after polishing, and the ceramic is placed in a resistance furnace. The temperature is kept at 850°C for 60 minutes, and the ceramic is naturally cooled to room temperature along with the furnace to obtain a piezoelectric ceramic plated with silver electrodes.

[0175] (9) Polarization

[0176] The silver-plated piezoelectric ceramic in step (8) is placed in silicone oil and polarized along the thickness direction using a DC electric field or an AC electric field. The polarization temperature is 150° C., the polarization voltage is 50 kV / cm, and the polarization voltage is maintained for 60 minutes to obtain a chemical formula of 0.19Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.2PbZrO3-0.6PbTiO3+0.01Pb(Mn 1 / 3 Nb 2 / 3 )O3 piezoelectric ceramics.

[0177] Example 6

[0178] Preparation of ceramic powder: For 0.01Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.6PbZrO3-0.3PbTiO3+0.09Pb(Mn 1 / 3Nb 2 / 3 )O3 samples, according to 0.01Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.6PbZrO3-0.3PbTiO3+0.09Pb(Mn 1 / 3 Nb 2 / 3 )O3 stoichiometric, weigh 67.1252g of PbO with a purity of 99.9%, 0.4962g of YbNbO4, 22.2349g of ZrO2 with a purity of 99.9%, 7.2057g of TiO2 with a purity of 99.9% and 3.0382g of MnNb2O6 as raw materials and mix them evenly to prepare

[0179] 0.01Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.6PbZrO3-0.3PbTiO3+0.09Pb(Mn 1 / 3 Nb 2 / 3 )O3 piezoelectric ceramic powder.

[0180] Tabletting: The ceramic powder after passing through an 80-mesh sieve is pressed into a cylindrical blank using a powder tablet press, and then cold isostatically pressed at a pressure of 200 MPa for 15 minutes.

[0181] Pressureless closed sintering: bury the cylindrical blank in homogeneous powder, place it on a zirconia plate, place the zirconia plate in an alumina closed sagger, heat it to 1100℃ at a heating rate of 2℃ / min, sinter for 3 hours, and cool it naturally to room temperature in the furnace to obtain the fired piezoelectric ceramics.

[0182] Polishing: The upper and lower surfaces of the sintered piezoelectric ceramics were polished with 600-grit sandpaper, and then polished with metallographic sandpaper to a thickness of 0.8 mm, and then ultrasonically cleaned with deionized water and ethanol, respectively, and dried.

[0183] Silver-plated electrode: Evenly coat the silver paste on the two polished surfaces of the ceramic, place it in a resistance furnace, keep it warm at 500°C for 5 minutes, and naturally cool it to room temperature with the furnace to obtain piezoelectric ceramics plated with silver electrodes.

[0184] Polarization: Place the silver-plated piezoelectric ceramic in silicone oil and polarize it along the thickness direction using a DC electric field or an AC electric field. The polarization temperature is 90°C, the polarization voltage is 10 kV / cm, and the polarization voltage is maintained for 10 minutes. The chemical formula is 0.01Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.6PbZrO3-0.3PbTiO3+0.09Pb(Mn 1 / 3 Nb 2 / 3 )O3 piezoelectric ceramics.

[0185] The other steps and process parameters are the same as those in Example 5.

[0186] Example 7

[0187] Preparation of ceramic powder: For 0.3Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.45PbZrO3-0.1PbTiO3+0.15Pb(Mn 1 / 3Nb 2 / 3 )O3 samples, according to 0.3Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.45PbZrO3-0.1PbTiO3+0.15Pb(Mn 1 / 3 Nb 2 / 3)O3 stoichiometric, weigh 63.2984g of PbO with a purity of 99.9%, 14.0362g of YbNbO4, 15.7255g of ZrO2 with a purity of 99.9%, 2.2650g of TiO2 with a purity of 99.9% and 64.7750g of MnNb2O as raw materials and mix them evenly to prepare

[0188] 0.3Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.45PbZrO3-0.1PbTiO3+0.15Pb(Mn 1 / 3 Nb 2 / 3 )O3 piezoelectric ceramic powder.

[0189] Tabletting: The ceramic powder after passing through a 150-mesh sieve is pressed into a cylindrical blank using a powder tablet press, and then cold isostatically pressed at a pressure of 300 MPa for 20 minutes.

[0190] Pressureless closed sintering: bury the cylindrical blank in homogeneous powder, place it on a zirconia plate, place the zirconia plate in an alumina closed sagger, heat it to 1300℃ at a heating rate of 2℃ / min, sinter it for 5 hours, and cool it naturally to room temperature in the furnace to obtain the fired piezoelectric ceramics.

[0191] Polishing: The upper and lower surfaces of the sintered piezoelectric ceramics were polished with 2000-grit sandpaper, and then polished with metallographic sandpaper to a thickness of 1 mm, and then ultrasonically cleaned with deionized water and ethanol, respectively, and dried.

[0192] Silver-plated electrode: Evenly coat the silver paste on the two polished surfaces of the ceramic, place it in a resistance furnace, keep it warm for 60 minutes at 650°C, and naturally cool it to room temperature with the furnace to obtain piezoelectric ceramics plated with silver electrodes.

[0193] Polarization: Place the silver-plated piezoelectric ceramic in silicone oil and polarize it along the thickness direction using a DC electric field or an AC electric field. The polarization temperature is 150°C, the polarization voltage is 50 kV / cm, and the polarization voltage is maintained for 60 minutes. The chemical formula is 0.3Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.45PbZrO3-0.1PbTiO3+0.15Pb(Mn 1 / 3 Nb 2 / 3 )O3 piezoelectric ceramics.

[0194] The other steps and process parameters are the same as those in Example 5.

[0195] Example 8

[0196] Preparation of ceramic powder: For 0.2Pb(Yb 1 / 2 Nb1 / 2 )O3-0.1PbZrO3-0.5PbTiO3+0.2Pb(Mn 1 / 3 Nb 2 / 3 )O3 samples, according to 0.2Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.1PbZrO3-0.5PbTiO3+0.2Pb(Mn 1 / 3 Nb 2 / 3 )O3 stoichiometric, weigh 99.9% pure PbO67.5197g, YbNbO49.9815g, 99.9% pure ZrO2 3.7276g, 99.9% pure TiO212.0800g and MnNb2O66.7813g as raw materials and mix them evenly to prepare

[0197] 0.2Pb(Yb 1 / 2 Nb 1 / 2 )O3-0.1PbZrO3-0.5PbTiO3+0.2Pb(Mn 1 / 3 Nb 2 / 3 )O3 piezoelectric ceramic powder.

[0198] The other steps and process parameters are the same as those in Example 5.

[0199] Figure 1 3 is a cross-sectional morphology of a scanning electron microscope (SEM) image of the PMnN-doped PYN-PZT piezoelectric ceramic prepared in Example 8. As shown in the figure, the prepared piezoelectric ceramic has uniform grain size and a dense structure.

[0200] Figure 2 This is a trend diagram of the dielectric constant of MnO2 and PMnN-doped PYN-PZT prepared in Examples 1, 2, 4, and 5 as a function of temperature. It can be seen from the figure that the prepared piezoelectric ceramics have a high Curie temperature (>370°C) and can be used in high temperature environments.

[0201] Figure 3 It is the hysteresis loop of the PYN-PZT piezoelectric ceramics prepared in Examples 3 and 6. It can be seen from the figure that under an electric field of 40kV / cm, the coercive field of the MnO2-doped PYN-PZT ceramics prepared in Example 3 is 25kV / cm, and the internal bias field is 5kV / cm; the coercive field of the PMnN-doped PYN-PZT ceramics prepared in Example 6 is 27kV / cm, and the internal bias field is 8.5kV / cm. A large coercive field can increase the withstand voltage threshold of the piezoelectric ceramics, making it suitable for high-power device applications. In addition, when the Mn doping content is the same, PMnN doping has a larger coercive field and internal bias field than MnO2 doping.

[0202] Figure 4The impedance diagram and phase angle of PMnN-doped PYN-PZT ceramic prepared in Example 6 are obtained by calculation. m Up to 3058, with excellent high-power performance.

[0203] Figure 5 is the vibration velocity of the PMnN-doped PYN-PZT ceramic prepared in Example 5. Under an AC electric field of 3 V / mm, the vibration velocity is about 0.95 m / s.

[0204] Figure 6 The figure shows the loss of MnO2 and PMnN doped PYN-PZT ceramics prepared in Examples 2 and 5 under strong AC electric field. The loss of MnO2 doped PYN-PZT ceramics gradually increases with the increase of the electric field, while the loss of PMnN doped PYN-PZT ceramics basically maintains a stable loss and is relatively low (~0.5%), indicating that it can be used in high-power environments driven by strong electric fields.

[0205] Figure 7 The XRD patterns of PYN-PZT, MnO2-doped PYN-PZT and PMnN-doped PYN-PZT piezoelectric ceramics are shown in Figure 2. Figure 7 It can be seen that PYN-PZT and Mn-doped PYN-PZT ceramics are pure perovskite structures without any second phase.

[0206] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A high-temperature piezoelectric ceramic for high-power scenarios, characterized in that: The high temperature piezoelectric ceramic is a Mn element doped lead zirconate titanate based piezoelectric ceramic; the lead zirconate titanate based is Pb(Yb 1 / 2 Nb 1 / 2 ) a three-phase solid solution of PbO3, PbZrO3 and PbTiO3; The doping method of the Mn element is metal oxide MnO2 doping or composite oxide Pb (Mn 1 / 3 Nb 2 / 3 )O3 doping.

2. The high-temperature piezoelectric ceramic for high-power scenarios according to claim 1, characterized in that: When the doping method of the Mn element is metal oxide MnO2 doping, the molecular formula of the Mn element doped lead zirconate titanate based piezoelectric ceramic is (1-xy)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zMnO2, wherein the value range of x is 0.1-0.6, the value range of y is 0.1-0.6, and the value range of z is 0.01-0.

1.

3. The high-temperature piezoelectric ceramic for high-power scenarios according to claim 1, characterized in that: The doping method of the Mn element is composite oxide Pb(Mn 1 / 3 Nb 2 / 3 )O3 doping, the molecular formula of the Mn element doped lead zirconate titanate based piezoelectric ceramic is (1-xyz)Pb(Yb 1 / 2 Nb 1 / 2 )O3-yPbZrO3-xPbTiO3+zPb(Mn 1 / 3 Nb 2 / 3 )O3, where x ranges from 0.1 to 0.6, y ranges from 0.1 to 0.6, and z ranges from 0.01 to 0.

2.

4. A method for preparing a high-temperature piezoelectric ceramic for high-power scenarios according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: preparing MnNb2O6 precursor powder or MnO2 and YbNbO4 precursor powder, mixing the ingredients according to the molecular formula of Mn element-doped lead zirconate titanate-based piezoelectric ceramics, and then ball milling, drying and sieving in sequence to obtain a raw material mixture; S2: The raw material mixture is pre-calcined and then cooled to room temperature, and then ground to obtain pre-calcined powder; S3: ball milling the calcined powder, followed by drying, grinding and sieving to obtain ceramic powder; S4: pressing the ceramic powder into a sheet to obtain a green piece, and then performing a pressureless closed sintering process on the green piece to obtain a fired piezoelectric ceramic; S5: The fired piezoelectric ceramics are polished, silver-plated, and polarized in sequence to obtain high-temperature piezoelectric ceramics for high-power scenarios.

5. The method for preparing high-temperature piezoelectric ceramics for high-power scenarios according to claim 4, characterized in that: When the Mn element is derived from the MnNb2O6 precursor powder, the Mn element in the lead zirconate titanate-based piezoelectric ceramics is doped in the form of a composite oxide Pb(Mn 1 / 3 Nb 2 / 3 )O3 doping; When the Mn element originates from MnO2, the doping mode of the Mn element in the Mn element-doped lead zirconate titanate-based piezoelectric ceramic is metal oxide MnO2 doping.

6. The method for preparing high-temperature piezoelectric ceramics for high-power scenarios according to claim 4, characterized in that: In S1, the preparation process of the MnNb2O6 precursor powder is as follows: MnO2 and Nb2O5 are taken according to the stoichiometric ratio of MnNb2O6 and mixed evenly, and then ball milled, dried, ground, and sieved in sequence. Finally, the mixture is calcined at a temperature of 1000°C to 1200°C to obtain MnNb2O6 precursor powder.

7. The method for preparing high-temperature piezoelectric ceramics for high-power scenarios according to claim 4, characterized in that: In S1, the preparation process of the YbNbO4 precursor powder is as follows: Yb2O3 and Nb2O5 are taken according to the stoichiometric ratio of YbNbO4 and mixed evenly, and then ball milled, dried, ground, and sieved in sequence, and then calcined at a temperature of 1000°C to 1100°C to synthesize YbNbO4 precursor powder.

8. The method for preparing high-temperature piezoelectric ceramics for high-power scenarios according to claim 4, characterized in that: In S2, the pre-burning process is as follows: The temperature is raised to 750°C to 850°C at a heating rate of 2 to 10°C / min and pre-fired for 2 to 5 hours.

9. The method for preparing high-temperature piezoelectric ceramics for high-power scenarios according to claim 4, characterized in that: In S4, the process of the pressureless closed sintering treatment is as follows: The blank is embedded in homogeneous ceramic powder and placed on a zirconia flat plate. The zirconia flat plate is placed in an alumina sealed sagger and heated to 1100-1300°C at a heating rate of 2-5°C / min. It is sintered for 3-5 hours and then naturally cooled to room temperature in the furnace.

10. The method for preparing high-temperature piezoelectric ceramics for high-power scenarios according to claim 4, characterized in that: In S5, the polishing process is as follows: The upper and lower surfaces of the fired piezoelectric ceramics were polished with 600-2000 grit sandpaper, and then polished with metallographic sandpaper to a thickness of 0.8-1.2 mm. The surfaces were then ultrasonically cleaned with deionized water and ethanol, and then dried. The silver plating process is as follows: The silver paste is evenly coated on the upper and lower surfaces of the polished fired piezoelectric ceramic, and then placed in a resistance furnace at a temperature of 500°C to 850°C for 5 minutes to 60 minutes, and then naturally cooled to room temperature along with the furnace; The polarization process is as follows: The silver-plated fired piezoelectric ceramic is placed in silicone oil and polarized along the thickness direction using a DC electric field or an AC electric field; the polarization temperature is 90°C to 150°C, the polarization voltage is 10kV / cm to 50kV / cm, and the polarization voltage is maintained for 10 to 60 minutes.

Citation Information

Patent Citations

  • Piezoelectric ceramic, piezoelectric element and piezoelectric device comprising piezoelectric element

    CN102557632A

  • Manganese niobate doped lead ytterbium niobate-lead zirconate titanate piezoelectric ceramic and preparation method thereof

    CN116675532A

  • PYN-PZT-based high-temperature texture piezoelectric ceramic, preparation method and application

    CN118184349A

  • Piezoelectric porcelain composition

    JP1995187778A

  • Piezoelectric ceramic, piezoelectric element with the same, piezoelectric device with the piezoelectric element

    JP2012076942A

Cited By

  • PZT-based texture piezoelectric ceramic as well as phase-change auxiliary polarization preparation method and application thereof

    CN121872799A

  • High-power piezoelectric ceramic as well as preparation method and application thereof