Method for preparing aluminum nitride ceramic through in-situ chemical deposition coating and aluminum nitride ceramic

By in-situ chemical deposition of coated yttrium oxide additives, the problem of low sintering activity of aluminum nitride ceramics is solved, and the preparation of aluminum nitride ceramics with high thermal conductivity and strength is achieved, which significantly improves its thermal and mechanical properties.

CN118930278APending Publication Date: 2024-11-12HUBEI XINZHONGDA SEMICONDUCTOR CO LTD

Patent Information

Application Number
CN202411108922.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The sintering activity of traditional aluminum nitride ceramics is low, resulting in poor thermal and mechanical properties. Especially during casting and forming, yttrium oxide sintering additives are difficult to play an effective role, affecting the forming performance of aluminum nitride ceramics.

Method used

Using in-situ chemical deposition coating method, yttrium salt is dissolved in ethanol and reacted with aluminum nitride powder, adjusted pH value and stirred at low temperature to form aluminum nitride powder with yttrium oxide on the surface, followed by solvent , dispersant and binder are mixed, and then formed by ball milling and casting, and finally aluminium nitride ceramic is produced by degreasing and sintering.

Benefits of technology

It significantly improves the mechanical and thermal properties of aluminum nitride ceramics, with thermal conductivity reaching 220W/m·K, flexural strength up to 360MPa, with more uniform microstructure, tight grain contact, low porosity, and better performance than traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930278A_ABST
    Figure CN118930278A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing aluminum nitride ceramic through in-situ chemical deposition coating and the aluminum nitride ceramic, and belongs to the technical field of ceramic tape casting. The preparation method of the aluminum nitride ceramic comprises the following steps: dissolving aluminum nitride powder in first ethanol, then continuously adding yttrium salt and a first dispersant, then adjusting the pH value to 6.5-10.5, and then stirring for reaction to obtain aluminum nitride powder coated with yttrium salt on the surface; calcining the aluminum nitride powder of which the surface is coated with the yttrium salt to obtain aluminum nitride powder of which the surface is coated with yttrium oxide in situ; mixing the aluminum nitride powder of which the surface is coated with yttrium oxide in situ, a solvent, a second dispersing agent, a plasticizer and a binder, and performing ball milling to obtain ceramic slurry; carrying out tape casting forming on the ceramic slurry through a tape casting forming machine to prepare an aluminum nitride ceramic green body; sequentially degreasing and sintering the aluminum nitride ceramic green body to obtain the aluminum nitride ceramic. The aluminum nitride ceramic obtained by the preparation method provided by the invention has excellent mechanical and thermal properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic tape casting, and in particular to a method for preparing aluminum nitride ceramics by in-situ chemical deposition coating and the aluminum nitride ceramics. Background Art

[0002] Aluminum Nitride Ceramic is a ceramic with aluminum nitride (AIN) as the main crystal phase. AIN crystal is a covalently bonded compound with (AIN4) tetrahedron as the structural unit, has a wurtzite structure, and belongs to the hexagonal crystal system. The chemical composition is Al 65.81%, N 34.19%, and the specific gravity is 3.261g / cm 3 , white or off-white, single crystal colorless and transparent, sublimation decomposition temperature under normal pressure is 2450℃. Aluminum nitride ceramic is a high temperature heat-resistant material. Thermal expansion coefficient (4.0-6.0)X10 -6 / ℃, the thermal conductivity of polycrystalline AIN reaches 260W / (mk). Aluminum nitride ceramic substrate has high thermal conductivity, low expansion coefficient, high strength, high temperature resistance, chemical corrosion resistance, high resistivity, and low dielectric loss. It is an ideal large-scale integrated circuit heat dissipation substrate and packaging material. Aluminum nitride ceramics are widely used in the field of modern electronic industry. Aluminum nitride ceramic substrate is the most widely used processing component of aluminum nitride ceramics. The most mainstream way to prepare aluminum nitride substrate is tape casting. Tape casting to prepare aluminum nitride not only has high processing efficiency, but also has high strength of the formed green body and strong machinability.

[0003] Aluminum nitride ceramics are typical non-oxide ceramics with low sintering activity. Pure aluminum nitride powder or tape-cast aluminum nitride ceramic greenware is difficult to sinter, and usually requires the addition of sintering aids. Yttrium oxide is the most important sintering aid for aluminum nitride ceramics, and plays a dual role in the sintering process. First, it combines with Al2O3 on the surface to form liquid aluminate. Under the action of viscous flow, it accelerates mass transfer, and the liquid phase fills the area around the grains. The original powder contact angle can be adjusted, and some pores are filled or discharged to promote sintering. At the same time, the sintering aid can react with oxygen to reduce the lattice oxygen content to obtain highly densified aluminum nitride ceramics. In the tape-casting process, the traditional mixing method of yttrium oxide sintering aid and aluminum nitride ceramic powder is mechanical dry mixing or alcohol wet mixing. However, in the ceramic slurry mixed by the traditional method, since the particle size of aluminum nitride and yttrium oxide powders is relatively fine, they are very easy to agglomerate in the slurry. As a result, during the sintering process of the tape-cast aluminum nitride green body, yttrium oxide is difficult to play a role on the surface of each aluminum nitride grain, seriously affecting the thermal and mechanical properties of the tape-cast aluminum nitride ceramics. Summary of the invention

[0004] The purpose of the present invention is to overcome the above technical deficiencies, provide a method for preparing aluminum nitride ceramics by in-situ chemical deposition coating and aluminum nitride ceramics, and solve the technical problem of how to obtain aluminum nitride ceramics with excellent thermal and mechanical properties in the prior art.

[0005] In order to achieve the above technical objectives, the technical solution of the present invention provides a method for preparing aluminum nitride ceramics by in-situ chemical deposition coating, comprising the following steps:

[0006] S1, dissolving aluminum nitride powder in a first ethanol, then continuing to add yttrium salt and a first dispersant, then adjusting the pH value to 6.5-10.5, and then stirring and reacting at 50-100° C. to obtain aluminum nitride powder with yttrium salt coated on the surface; calcining the aluminum nitride powder with yttrium salt coated on the surface at 300-600° C. to obtain aluminum nitride powder with yttrium oxide in-situ coated on the surface;

[0007] S2, mixing the aluminum nitride powder with yttrium oxide in-situ coated on the surface, a solvent, a second dispersant, a plasticizer and a binder, and ball-milling the mixture to obtain a ceramic slurry;

[0008] S3, tape-casting the ceramic slurry by a tape-casting machine to obtain an aluminum nitride ceramic green body;

[0009] S4. Degreasing and sintering the aluminum nitride ceramic green body in sequence to obtain aluminum nitride ceramic; the degreasing rate is 0.1-0.5°C / min, the insulation temperature is 280-300°C, 350-380°C, 400-450°C, 580-600°C, and the insulation time is 60-180min; the sintering temperature is 1850-1950°C, and the sintering time is 120-240min.

[0010] In any embodiment, in step S1, the yttrium salt is one or more of yttrium nitrate, yttrium sulfate and yttrium chloride; and / or the first dispersant is one or more of oleic acid, stearic acid and ammonium polyacrylate; the addition amount of the first dispersant is 2-5% of the mass of the ceramic powder.

[0011] In any embodiment, in step S1, the mass ratio of the aluminum nitride powder to the first ethanol is 1:(10-30); and / or, the calcination time is 120-240 min.

[0012] In any embodiment, in step S1, the stirring reaction time at 50-100° C. is 4-8 h, and the stirring speed of the stirring reaction is 400-800 rpm.

[0013] In any embodiment, in step S2, the solvent is a mixture of a second ethanol and butanone, and the volume ratio of the second ethanol to the butanone is (4-7):(3-6); the mass ratio of the aluminum nitride powder, the solvent, the second dispersant, the plasticizer and the binder is 50:(25-28):(2-4):(15-17):(8-10).

[0014] In any embodiment, in step S2, the second dispersant is a polymer copolymer dispersant, and the polymer copolymer dispersant is one or both of BYK111 and BYK163.

[0015] In any embodiment, in step S2, the plasticizer is one or both of polypropylene glycol 400 and dibutyl phthalate; and / or the binder is polyvinyl butyral.

[0016] In any embodiment, in step S2, the ball mill used in the ball milling is a plastic ball mill, the ball-to-material mass ratio is 2:(1-1.5), the ball milling speed is 400-800 rpm, and the ball milling time is 12-18 h.

[0017] In any embodiment, in step S3, the temperature of the tape casting is 60-80°C, the tape speed is 40-100 mm / s, and the tape thickness is 100-300 μm.

[0018] In addition, the present invention also provides an aluminum nitride ceramic, which is prepared by the above-mentioned method for preparing the aluminum nitride ceramic by in-situ chemical deposition coating.

[0019] Compared with the prior art, the beneficial effects of the present invention include: the present invention provides a method for preparing aluminum nitride ceramics, comprising the following steps: S1, dissolving aluminum nitride powder in a first ethanol, then continuing to add yttrium salt and a first dispersant, then adjusting the pH value to 6.5-10.5, and then stirring the reaction at 50-100° C. to obtain aluminum nitride powder with yttrium salt coated on the surface; calcining the aluminum nitride powder with yttrium salt coated on the surface at 300-600° C. to obtain aluminum nitride powder with yttrium oxide in-situ coated on the surface; S2, mixing the aluminum nitride powder with yttrium oxide in-situ coated on the surface, a solvent, and a second dispersant; The agent, plasticizer and binder are mixed and ball-milled to obtain ceramic slurry; S3, the ceramic slurry is tape-casted by a tape-casting machine to obtain aluminum nitride ceramic green body; S4, the aluminum nitride ceramic green body is degreased and sintered in sequence to obtain aluminum nitride ceramic; the degreasing rate is 0.1-0.5℃ / min, the insulation temperature is 280-300℃, 350-380℃, 400-450℃, 580-600℃, and the insulation time is 60-180min; the sintering temperature is 1850-1950℃, and the sintering time is 120-240min. The aluminum nitride ceramic obtained by the preparation method proposed in the present invention has excellent mechanical and thermal properties, and the thermal conductivity of the aluminum nitride ceramic is as high as 220W / m℃, and the flexural strength is as high as 360MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a SEM image of the aluminum nitride ceramic prepared in Example 1 of the present invention.

[0021] Figure 2 It is a SEM picture of the aluminum nitride ceramic prepared in Comparative Example 1 of the present invention.

[0022] Figure 3 It is a SEM picture of the aluminum nitride ceramic prepared in Comparative Example 2 of the present invention.

[0023] Figure 4 These are the test results of mechanical and thermal properties of aluminum nitride ceramics prepared in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0024] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0025] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0026] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0027] This specific embodiment provides a method for preparing aluminum nitride ceramics by in-situ chemical deposition coating, comprising the following steps:

[0028] S1, dissolving aluminum nitride powder in a first ethanol, then continuing to add yttrium salt and a first dispersant, then adjusting the pH value to 6.5-10.5, and then stirring the reaction at 50-100°C for 4-8h to obtain aluminum nitride powder with a surface coated with yttrium salt; the yttrium salt is one or more of yttrium nitrate, yttrium sulfate and yttrium chloride; the first dispersant is one or more of oleic acid, stearic acid and ammonium polyacrylate, and the addition amount of the first dispersant is 2-5% of the mass of the ceramic powder; the mass ratio of the aluminum nitride powder to the first ethanol is 1:(10-30); the stirring speed of the stirring reaction is 400-800rpm;

[0029] S2, the aluminum nitride powder coated with yttrium salt, a solvent, a second dispersant, a plasticizer and a binder are mixed and ball-milled to obtain a ceramic slurry; the solvent is a mixture of a second ethanol and butanone, and the volume ratio of the second ethanol to the butanone is (4-7):(3-6); the mass ratio of the aluminum nitride powder, the solvent, the second dispersant, the plasticizer and the binder is 50:(25-28):(2-4):(15-17):(8-10) The second dispersant is a polymer copolymer dispersant, and the polymer copolymer dispersant is one or both of BYK111 and BYK163; the plasticizer is one or both of polypropylene glycol 400 and dibutyl phthalate; the binder is polyvinyl butyral ester; the ball mill used in the ball milling is a plastic ball mill, the ball-to-material mass ratio is 2:(1-1.5), the ball milling speed is 400-800rpm, and the ball milling time is 12-18h;

[0030] S3, tape-casting the ceramic slurry through a tape-casting machine to obtain an aluminum nitride ceramic green body; the tape-casting temperature is 60-80° C., the tape speed is 40-100 mm / s, and the tape thickness is 100-300 μm;

[0031] S4. Degreasing and sintering the aluminum nitride ceramic green body in sequence to obtain aluminum nitride ceramic, wherein the degreasing rate is 0.1-0.5°C / min, the insulation temperature is 280-300°C, 350-380°C, 400-450°C, 580-600°C, and the insulation time is 60-180min; the sintering temperature is 1850-1950°C, and the sintering time is 120-240min.

[0032] This specific embodiment also provides an aluminum nitride ceramic, which is prepared by the above-mentioned method for preparing aluminum nitride ceramic by in-situ chemical deposition coating.

[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0034] In the present invention, reference is made to “some embodiments”, “this embodiment”, examples, etc., which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.

[0035] If similar descriptions of "first / second" appear in the application documents, the following instructions are added. In the following description, the terms "first\second\third" involved are merely used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged in a specific order or sequence where permitted, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein.

[0036] In this embodiment, the term "and / or" is merely a description of the association relationship between associated objects, indicating that three relationships may exist. For example, object A and / or object B may represent three situations: object A exists alone, object A and object B exist at the same time, and object B exists alone.

[0037] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0038] The polymer copolymer dispersants in the following examples are BYK111 and BYK163 purchased from BYK Chemicals GmbH, Germany.

[0039] Example 1

[0040] This embodiment provides an aluminum nitride ceramic, which is prepared by the following steps:

[0041] S1. Dissolve aluminum nitride powder in an ethanol solution with a mass concentration of 30%, stir at high speed at 60°C, the mass ratio of aluminum nitride powder to ethanol is 1:10, seal and stir, and the stirring speed is 200rpm; then continue to add yttrium nitrate solution and oleic acid to the above-mentioned ethanol molten salt containing aluminum nitride, the concentration of yttrium nitrate solution is 5g / L, the addition amount of the yttrium nitrate solution is 40% of the mass of the ethanol molten salt, and the addition amount of oleic acid is 3% of the mass of the ceramic powder, adjust the pH value to 7, stir at 80°C, the stirring speed is 800rpm, and the stirring time is 6h to obtain aluminum nitride powder with yttrium salt coated on the surface; calcine the aluminum nitride powder with yttrium salt coated on the surface in air atmosphere, the calcination temperature is 600°C, and the calcination time is 150min to obtain aluminum nitride powder with yttrium oxide coated on the surface in situ;

[0042] S2, the aluminum nitride powder with yttrium oxide in-situ coated on the surface, solvent, BYK111 polymer copolymer dispersant, polypropylene glycol 400, and polyvinyl butyral ester PVB are mixed and ball-milled to obtain a ceramic slurry; the solvent is a mixture of ethanol and butanone, the volume ratio of ethanol to butanone is 7:3, the ball mill is a plastic ball mill, the ball-to-material mass ratio is 2:1, the ball milling speed is 400 rpm, and the ball milling time is 15 hours; the mass ratio of the aluminum nitride powder, the solvent, the BYK111 polymer copolymer dispersant, polypropylene glycol 400 and polyvinyl butyral ester PVB is 50:25:2:15:9;

[0043] S3, tape-casting the ceramic slurry through a tape-casting machine to obtain an aluminum nitride ceramic green body, the tape-casting temperature is 80° C., the tape speed is 50 mm / s, the tape thickness is 200 μm, and a single-layer aluminum nitride thin layer is obtained;

[0044] S4. Degreasing and sintering the aluminum nitride ceramic green body in sequence to obtain aluminum nitride ceramic, with a degreasing rate of 0.5°C / min, holding temperatures of 280, 380, 450, and 600°C, a holding time of 120 min, a sintering temperature of 1850°C, and a sintering time of 120 min.

[0045] Example 2

[0046] This embodiment provides an aluminum nitride ceramic, which is prepared by the following steps:

[0047] S1. Dissolve aluminum nitride powder in an ethanol solution with a mass concentration of 20%, stir at a high speed at 50°C, the mass ratio of aluminum nitride powder to ethanol is 1:20, stir in a sealed state, and the stirring speed is 400rpm; then continue to add yttrium sulfate solution and oleic acid to the above-mentioned ethanol molten salt containing aluminum nitride, the concentration of yttrium nitrate solution is 2g / L, the addition amount of the yttrium nitrate solution is 50% of the mass of the ethanol molten salt, and the addition amount of the oleic acid is 3% of the mass of the ceramic powder, adjust the pH value to 6.5, stir at 70°C, the stirring speed is 600rpm, and the stirring time is 4h to obtain aluminum nitride powder with yttrium salt coated on the surface; calcine the aluminum nitride powder with yttrium salt coated on the surface in an air atmosphere, the calcination temperature is 450°C, and the calcination time is 120min to obtain aluminum nitride powder with yttrium oxide coated on the surface in situ;

[0048] S2, mixing the aluminum nitride powder with yttrium oxide in-situ coated on the surface, solvent, BYK163 polymer copolymer dispersant, dibutyl phthalate, and polyvinyl butyral ester (PVB) and ball milling to obtain a ceramic slurry; the solvent is a mixture of ethanol and butanone, the volume ratio of ethanol to butanone is 7:3, the ball mill is a plastic ball mill, the ball-to-material mass ratio is 2:1, the ball milling speed is 600 rpm, and the ball milling time is 18 hours; the mass ratio of the aluminum nitride powder, the solvent, the BYK163 polymer copolymer dispersant, dibutyl phthalate and polyvinyl butyral ester (PVB) is 50:26:3:16:8;

[0049] S3, tape-casting the ceramic slurry through a tape-casting machine to obtain an aluminum nitride ceramic green body, the tape-casting temperature is 60° C., the tape speed is 100 mm / s, the tape thickness is 260 μm, and a single-layer aluminum nitride thin layer is obtained;

[0050] S4. Degreasing and sintering the aluminum nitride ceramic green body in sequence to obtain aluminum nitride ceramic, with a degreasing rate of 0.2°C / min, holding temperatures of 280, 380, 450, and 600°C, a holding time of 180 min, a sintering temperature of 1900°C, and a sintering time of 120 min.

[0051] Example 3

[0052] This embodiment provides an aluminum nitride ceramic, which is prepared by the following steps:

[0053] S1. Dissolve aluminum nitride powder in an ethanol solution with a mass concentration of 40%, stir at high speed at 60°C, the mass ratio of aluminum nitride powder to ethanol is 1:30, seal and stir, and the stirring speed is 300rpm; then continue to add yttrium nitrate solution and oleic acid to the above-mentioned ethanol molten salt containing aluminum nitride, the concentration of yttrium nitrate solution is 10g / L, the addition amount of the yttrium nitrate solution is 30% of the mass of the ethanol molten salt, and the addition amount of oleic acid is 3% of the mass of the ceramic powder, adjust the pH value to 8, stir at 70°C, the stirring speed is 600rpm, and the stirring time is 5h to obtain aluminum nitride powder with yttrium salt coated on the surface; calcine the aluminum nitride powder with yttrium salt coated on the surface in air atmosphere, the calcination temperature is 500°C, and the calcination time is 120min to obtain aluminum nitride powder with yttrium oxide coated on the surface in situ;

[0054] S2, the aluminum nitride powder with yttrium oxide in-situ coated on the surface, solvent, BYK111 polymer copolymer dispersant, polypropylene glycol 400, and polyvinyl butyral ester PVB are mixed and ball-milled to obtain a ceramic slurry; the solvent is a mixture of ethanol and butanone, the volume ratio of ethanol to butanone is 2:3, the ball mill is a plastic ball mill, the ball-to-material mass ratio is 2:1, the ball milling speed is 600 rpm, and the ball milling time is 12 h; the mass ratio of the aluminum nitride powder, the solvent, the BYK111 polymer copolymer dispersant, polypropylene glycol 400 and polyvinyl butyral ester PVB is 50:28:4:17:10;

[0055] S3, tape-casting the ceramic slurry through a tape-casting machine to obtain an aluminum nitride ceramic green body, the tape-casting temperature is 60° C., the tape speed is 100 mm / s, the tape thickness is 220 μm, and a single-layer aluminum nitride thin layer is obtained;

[0056] S4. Degreasing and sintering the aluminum nitride ceramic green body in sequence to obtain aluminum nitride ceramic, with a degreasing rate of 0.15°C / min, holding temperatures of 280, 380, 450, and 600°C, a holding time of 120 min, a sintering temperature of 1900°C, and a sintering time of 150 min.

[0057] Example 4

[0058] This embodiment provides an aluminum nitride ceramic, which is prepared by the following steps:

[0059] S1. Dissolve aluminum nitride powder in an ethanol solution with a mass concentration of 30%, stir at high speed at 100°C, the mass ratio of aluminum nitride powder to ethanol is 1:30, seal and stir, and the stirring speed is 300rpm; then continue to add yttrium chloride solution and oleic acid to the above-mentioned ethanol molten salt containing aluminum nitride, the concentration of yttrium nitrate solution is 6g / L, the addition amount of the yttrium nitrate solution is 35% of the mass of the ethanol molten salt, and the addition amount of oleic acid is 3% of the mass of the ceramic powder, adjust the pH value to 10.5, stir at 100°C, the stirring speed is 600rpm, and the stirring time is 4h to obtain aluminum nitride powder with yttrium salt coated on the surface; calcine the aluminum nitride powder with yttrium salt coated on the surface in air atmosphere, the calcination temperature is 300°C, and the calcination time is 120min to obtain aluminum nitride powder with yttrium oxide coated on the surface in situ;

[0060] S2, the aluminum nitride powder with yttrium oxide in-situ coated on the surface, solvent, BYK111 polymer copolymer dispersant, polypropylene glycol 400, and polyvinyl butyral ester PVB are mixed and ball-milled to obtain a ceramic slurry; the solvent is a mixture of ethanol and butanone, the volume ratio of ethanol to butanone is 5:4, the ball mill is a plastic ball mill, the ball-to-material mass ratio is 2:1, the ball milling speed is 600 rpm, and the ball milling time is 15 hours; the mass ratio of the aluminum nitride powder, the solvent, the BYK111 polymer copolymer dispersant, polypropylene glycol 400 and polyvinyl butyral ester PVB is 50:27:4:17:8;

[0061] S3, tape-casting the ceramic slurry through a tape-casting machine to obtain an aluminum nitride ceramic green body, the tape-casting temperature is 70° C., the tape speed is 40 mm / s, the tape thickness is 100 μm, and a single-layer aluminum nitride thin layer is obtained;

[0062] S4. Degreasing and sintering the aluminum nitride ceramic green body in sequence to obtain aluminum nitride ceramic, with a degreasing rate of 0.5°C / min, holding temperatures of 280, 380, 450, and 600°C, a holding time of 60 min, a sintering temperature of 1850°C, and a sintering time of 240 min.

[0063] Comparative Example 1

[0064] The difference between the preparation method of aluminum nitride ceramic in this comparative example and that in Example 1 is that in step S1, no calcination treatment is performed, which is as follows:

[0065] S1. Dissolve aluminum nitride powder in an ethanol solution with a mass concentration of 30%, stir evenly at a high speed at 60°C, the mass ratio of aluminum nitride powder to ethanol is 1:10, seal and stir, and the stirring speed is 200rpm; then continue to add yttrium nitrate solution and oleic acid to the above-mentioned ethanol molten salt containing aluminum nitride, the concentration of yttrium nitrate solution is 5g / L, the addition amount of the yttrium nitrate solution is 40% of the mass of the ethanol molten salt, and the addition amount of the oleic acid is 3% of the mass of the ceramic powder, adjust the pH value to 7, stir evenly at 80°C, the stirring speed is 800rpm, and the stirring time is 6h to obtain aluminum nitride powder coated with yttrium salt on the surface;

[0066] S2, the aluminum nitride powder coated with yttrium salt on the surface, solvent, BYK111 polymer copolymer dispersant, polypropylene glycol 400, and polyvinyl butyral ester PVB are mixed and ball-milled to obtain a ceramic slurry; the solvent is a mixture of ethanol and butanone, the volume ratio of ethanol to butanone is 7:3, the ball mill is a plastic ball mill, the ball-to-material mass ratio is 2:1, the ball milling speed is 400 rpm, and the ball milling time is 15 hours; the mass ratio of the aluminum nitride powder, the solvent, the BYK111 polymer copolymer dispersant, polypropylene glycol 400 and polyvinyl butyral ester PVB is 50:25:2:15:9;

[0067] S3, tape-casting the ceramic slurry through a tape-casting machine to obtain an aluminum nitride ceramic green body, the tape-casting temperature is 80° C., the tape speed is 50 mm / s, the tape thickness is 200 μm, and a single-layer aluminum nitride thin layer is obtained;

[0068] S4. Degreasing and sintering the aluminum nitride ceramic green body in sequence to obtain aluminum nitride ceramic, with a degreasing rate of 0.5°C / min, holding temperatures of 280, 380, 450, and 600°C, a holding time of 120 min, a sintering temperature of 1850°C, and a sintering time of 120 min.

[0069] Comparative Example 2

[0070] The difference between the preparation method of aluminum nitride ceramic in this comparative example and that in Example 1 is that the processing steps of step S1 are different, as follows:

[0071] S1. Dry-mixing aluminum nitride powder and yttrium oxide powder by ball milling according to the amounts of aluminum and yttrium in Example 1 to obtain composite aluminum nitride ceramic powder;

[0072] S2, the composite aluminum nitride ceramic powder, solvent, BYK111 polymer copolymer dispersant, polypropylene glycol 400, and polyvinyl butyral ester PVB are mixed and ball-milled to obtain a ceramic slurry; the solvent is a mixture of ethanol and butanone, the volume ratio of ethanol to butanone is 7:3, the ball mill is a plastic ball mill, the ball-to-material mass ratio is 2:1, the ball milling speed is 400 rpm, and the ball milling time is 15 hours; the mass ratio of the aluminum nitride powder, the solvent, the BYK111 polymer copolymer dispersant, polypropylene glycol 400 and polyvinyl butyral ester PVB is 50:25:2:15:9;

[0073] S3, tape-casting the ceramic slurry through a tape-casting machine to obtain an aluminum nitride ceramic green body, the tape-casting temperature is 80° C., the tape speed is 50 mm / s, the tape thickness is 200 μm, and a single-layer aluminum nitride thin layer is obtained;

[0074] S4. Degreasing and sintering the aluminum nitride ceramic green body in sequence to obtain aluminum nitride ceramic, with a degreasing rate of 0.5°C / min, holding temperatures of 280, 380, 450, and 600°C, a holding time of 120 min, a sintering temperature of 1850°C, and a sintering time of 120 min.

[0075] Combination Figure 1 , Figure 2 and Figure 3 It can be seen that the aluminum nitride grain size in the aluminum nitride ceramics obtained in Comparative Examples 1 and 2 is uneven, obvious pores are observed, and the grains are not in close contact, while the aluminum nitride ceramics obtained in Example 1 have uniform aluminum nitride grain size, low porosity, and close grain contact.

[0076] The flexural strength and thermal conductivity of the aluminum nitride ceramics prepared in Example 1, Comparative Example 1 and Comparative Example 2 were tested according to GB / T 3962-2017 and GB / T 39862-2021. The results are as follows: Figure 4 As shown, from Figure 4 It can be seen that the thermal conductivity of the aluminum nitride ceramic prepared in Example 1 is 220 W / m°C, and the flexural strength is 360 MPa; the thermal conductivity of the aluminum nitride ceramic prepared in Comparative Example 1 is 185 W / m°C, and the flexural strength is 270 MPa; the thermal conductivity of the aluminum nitride ceramic prepared in Comparative Example 2 is 148 W / m°C, and the flexural strength is 200 MPa; it can be seen that the thermal properties and mechanical properties of the aluminum nitride ceramic of Example 1 are significantly better than those of Comparative Examples 1 and 2.

[0077] It should be noted that the thermal properties and mechanical properties of the aluminum nitride ceramics prepared in Examples 2-4 of the present invention are equivalent to those in Example 1.

[0078] Other beneficial effects of the present invention:

[0079] 1) By in-situ depositing yttrium oxide sintering aid on aluminum nitride ceramic powder, the yttrium oxide sintering aid and aluminum nitride ceramic molecules are uniformly mixed at the molecular scale, and the function of the yttrium oxide sintering aid is maximized. The microstructure of aluminum nitride ceramics sintered by tape casting is more uniform than that of aluminum nitride ceramics made by traditional mechanical dry mixing or solvent wet mixing, with obvious grain refinement, and greatly improved mechanical and thermal properties.

[0080] 2) By in-situ chemical deposition of yttrium oxide on the surface of aluminum nitride powder, the deposition amount of yttrium oxide powder on the surface of aluminum nitride powder can be controlled by controlling the concentration of yttrium salt molten salt, thereby accurately controlling the amount of yttrium oxide sintering aid added, thereby preventing the problem of insufficient sintering aid function caused by insufficient yttrium oxide addition or increased liquid phase content and decreased sintering performance caused by excessive yttrium oxide addition.

[0081] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing aluminum nitride ceramics by in-situ chemical deposition coating, characterized in that: The following steps are involved: S1, dissolving aluminum nitride powder in a first ethanol, then continuing to add yttrium salt and a first dispersant, then adjusting the pH value to 6.5-10.5, and then stirring and reacting at 50-100° C. to obtain aluminum nitride powder with yttrium salt coated on the surface; calcining the aluminum nitride powder with yttrium salt coated on the surface at 300-600° C. to obtain aluminum nitride powder with yttrium oxide in-situ coated on the surface; S2, mixing the aluminum nitride powder with yttrium oxide in-situ coated on the surface, a solvent, a second dispersant, a plasticizer and a binder, and ball-milling the mixture to obtain a ceramic slurry; S3, tape-casting the ceramic slurry by a tape-casting machine to obtain an aluminum nitride ceramic green body; S4. Degreasing and sintering the aluminum nitride ceramic green body in sequence to obtain aluminum nitride ceramic; the degreasing rate is 0.1-0.5°C / min, the insulation temperature is 280-300°C, 350-380°C, 400-450°C, 580-600°C, and the insulation time is 60-180min; the sintering temperature is 1850-1950°C, and the sintering time is 120-240min.

2. The method for preparing aluminum nitride ceramics by in-situ chemical deposition coating according to claim 1, characterized in that: In step S1, the yttrium salt is one or more of yttrium nitrate, yttrium sulfate and yttrium chloride; and / or the first dispersant is one or more of oleic acid, stearic acid and ammonium polyacrylate; the addition amount of the first dispersant is 2-5% of the mass of the ceramic powder.

3. The method for preparing aluminum nitride ceramics by in-situ chemical deposition coating according to claim 1, characterized in that: In step S1, the mass ratio of the aluminum nitride powder to the first ethanol is 1:(10-30); and / or the calcination time is 120-240 min.

4. The method for preparing aluminum nitride ceramics by in-situ chemical deposition coating according to claim 1, characterized in that: In step S1, the stirring reaction time is 4-8 hours at 50-100° C., and the stirring speed is 400-800 rpm.

5. The method for preparing aluminum nitride ceramics by in-situ chemical deposition coating according to claim 1, characterized in that: In step S2, the solvent is a mixture of a second ethanol and butanone, and the volume ratio of the second ethanol to the butanone is (4-7):(3-6); the mass ratio of the aluminum nitride powder, the solvent, the second dispersant, the plasticizer and the binder is 50:(25-28):(2-4):(15-17):(8-10).

6. The method for preparing aluminum nitride ceramics by in-situ chemical deposition coating according to claim 1, characterized in that: In step S2, the second dispersant is a polymer copolymer dispersant, and the polymer copolymer dispersant is one or both of BYK111 and BYK163.

7. The method for preparing aluminum nitride ceramics by in-situ chemical deposition coating according to claim 1, characterized in that: In step S2, the plasticizer is one or both of polypropylene glycol 400 and dibutyl phthalate; and / or the binder is polyvinyl butyral.

8. The method for preparing aluminum nitride ceramics by in-situ chemical deposition coating according to claim 1, characterized in that: In step S2, the ball mill used in the ball milling is a plastic ball mill, the ball-to-material mass ratio is 2:(1-1.5), the ball milling speed is 400-800 rpm, and the ball milling time is 12-18 hours.

9. The method for preparing aluminum nitride ceramics by in-situ chemical deposition coating according to claim 1, characterized in that: In step S3, the temperature of the tape casting is 60-80°C, the tape speed is 40-100 mm / s, and the tape thickness is 100-300 μm.

10. An aluminum nitride ceramic, characterized in that: The aluminum nitride ceramic is prepared by the method for preparing the aluminum nitride ceramic by in-situ chemical deposition coating as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Film coated nitride ceramic composite powder, preparation method thereof, and nitride ceramic part and preparation method thereof

    CN110395994A

  • Preparation method of coated aluminum nitride powder and prepared aluminum nitride ceramic substrate

    CN113185303A

Cited By

  • High-strength aluminum nitride substrate and preparation method thereof

    CN122647239A