Method for preparing foamed ceramic filter by using waste chrome corundum

By grinding and sieving waste chromium corundum, and forming complex oxides with nano lanthanum oxide, nano cerium oxide and sodium dodecylbenzene sulfonate, combining isothiazolinone derivatives and ammonium carbonate as additives, Preparing foam ceramic filters solves the problem of waste chromium corundum in foam ceramics and improves the filtration effect and service life.

CN118930310AActive Publication Date: 2024-11-12JIANGXI HONGKE SPECIAL ALLOYS +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411140813.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Waste chromium corundum cannot be used directly to prepare foam ceramics, resulting in small amount of addition, poor filtration effect, easy introduction of chromium impurities and short service life.

Method used

By grinding and sieving waste chromium corundum, mixing nano lanthanum oxide, nano cerium oxide and sodium dodecylbenzenesulfonate to form complex oxides, combining isothiazolinone derivatives and ammonium carbonate as additives, foam ceramics are prepared Filter.

Benefits of technology

It effectively avoids chromium pollution, improves the filtration effect and service life, solves the problems of chromium pollution and poor filtration effect, and enhances the structural stability of the filter.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000737170000021
    Figure BDA0005000737170000021
  • Figure BDA0005000737170000051
    Figure BDA0005000737170000051
  • Figure BDA0005000737170000061
    Figure BDA0005000737170000061
Patent Text Reader

Abstract

The invention provides a method for preparing a foamed ceramic filter from waste chrome corundum, and relates to the field of foamed ceramics. The method comprises the following steps: grinding the waste chrome corundum, and screening by a 200-mesh sieve to obtain screen underflow; mixing the first raw materials, sintering, and then cooling and crushing to obtain first powder; the first raw material is prepared from 95 to 97 percent of screen underflow, 1 to 2 percent of nano lanthanum oxide, 1 to 2 percent of nano cerium oxide, 0.5 to 1 percent of sodium dodecyl benzene sulfonate and 0.1 to 0.5 percent of K4Sb2O7; mixing the second raw materials, adding water and stirring to obtain slurry; the second raw material comprises 50-70% of first powder, 20-40% of aluminum oxide, 5-10% of zirconium oxide, 1-5% of an isothiazolinone derivative and 1-5% of ammonium carbonate; dipping the carrier in the slurry, extruding and drying to obtain a blank; sintering and cooling the blank to obtain the foamed ceramic filter. According to the method provided by the invention, the foamed ceramic filter can be prepared from the waste chrome corundum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of foam ceramics, and in particular to a method for preparing a foam ceramic filter by utilizing waste chromium corundum. Background Art

[0002] The main mineral composition of chrome corundum is α-Al 2 O 3 -Cr 2 O 3 Solid solution. Waste chrome corundum mainly comes from glass kiln linings, drawn glass flow hole cover bricks and waste refractory materials used for molten iron pretreatment devices, waste incinerators, and water-coal slurry pressurized gasification furnace backings.

[0003] The main raw material of foam ceramics is alumina, and waste chrome corundum contains a large amount of alumina. Therefore, recycling waste chrome corundum to prepare foam ceramics is one of the ways to reuse it as a resource.

[0004] However, waste chromium corundum cannot be used directly to prepare foam ceramics. Even if it is reluctantly added to the raw materials, there are often problems such as small addition amount, poor filtration effect, easy introduction of impurity elements such as chromium, and short service life.

[0005] Therefore, it is necessary to study a method to solve the above problems and realize the effective utilization of waste chrome corundum. Summary of the invention

[0006] The purpose of this application is to provide a method for preparing a foam ceramic filter using waste chromium corundum to solve the above problems.

[0007] To achieve the above objectives, this application adopts the following technical solutions:

[0008] A method for preparing a foam ceramic filter using waste chromium corundum comprises:

[0009] Grinding the waste chrome corundum, and then sieving it with a 200-mesh sieve to obtain the undersize;

[0010] The first raw materials are mixed, first sintered, and then first cooled and first crushed to obtain a first powder; the first raw materials, calculated with their total mass as 100%, include: 95-97% of the undersize, 1-2% of nano lanthanum oxide, 1-2% of nano cerium oxide, 0.5-1% of sodium dodecylbenzene sulfonate, K 4 Sb 2 O 7 0.1-0.5%;

[0011] Sodium dodecylbenzene sulfonate is usually used as a surfactant, but in this application, it is mainly used as a catalyst to promote the reaction of waste chromium corundum and lanthanum oxide, cerium oxide, K 4 Sb 2O 7 The complex oxide is formed, thereby solidifying the chromium element and preventing it from melting out of the filter during the subsequent sintering process and use, thereby contaminating the filtrate.

[0012] Optionally, the first raw material is calculated with its total mass as 100%, and the amount of the undersize can be 95%, 96%, 97% or any value between 95-97%; the amount of nano lanthanum oxide can be 1%, 1.5%, 2% or any value between 1-2%; the amount of nano cerium oxide can be 1%, 1.5%, 2% or any value between 1-2%; the amount of sodium dodecylbenzene sulfonate can be 0.5%, 06%, 0.7%, 0.8%, 0.9%, 1% or any value between 0.5-1%; K 4 Sb 2 O 7 The dosage can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5% or any value between 0.1-0.5%.

[0013] The second raw material is mixed, and water is added and stirred to prepare a slurry; the second raw material, calculated based on its own total mass as 100%, includes: 50-70% of the first powder, 20-40% of aluminum oxide, 5-10% of zirconium oxide, 1-5% of isothiazolinone derivative, and 1-5% of ammonium carbonate; the structural formula of the isothiazolinone derivative is:

[0014]

[0015] The slurry is impregnated into a soft polyurethane foam as a carrier, and then extruded and dried to obtain a blank;

[0016] The blank is subjected to a second sintering and a second cooling to obtain a foam ceramic filter.

[0017] It should be noted that the preparation method of the isothiazolinone derivative refers to existing literature, which specifically includes: reacting NaH, N,N-dimethylformamide and isothiazolin-3-one under a protective atmosphere, adding γ-chloropropyltriethoxysilane, first reacting under ice bath conditions for 20-40 minutes, then reacting at 70-100°C for 2-4 hours, and then separating the solvent to obtain the target substance.

[0018] The role of ammonium carbonate is to compensate for the defect of decreased filtering effect after using isothiazolinone derivatives.

[0019] Optionally, the second raw material is calculated with its total mass as 100%, and the amount of the first powder can be 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70% or any value between 50-70%; the amount of alumina can be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40% or any value between 20-40%; the amount of zirconium oxide can be 5%, 6%, 7%, 8%, 9%, 10% or any value between 5-10%; the amount of isothiazolinone derivative can be 1%, 2%, 3%, 4%, 5% or any value between 1-5%; the amount of ammonium carbonate can be 1%, 2%, 3%, 4%, 5% or any value between 1-5%.

[0020] Preferably, the first sintering is performed at a temperature of 1100-1300° C. and for a time of 3-6 hours.

[0021] Optionally, the first sintering temperature may be 1100° C., 1200° C., 1300° C. or any value between 1100-1300° C., and the sintering time may be 3 h, 4 h, 5 h, 6 h or any value between 3-6 h.

[0022] Preferably, the second sintering is performed at a temperature of 1200-1400° C. and for a time of 1-5 h.

[0023] Optionally, the temperature of the second sintering may be 1200° C., 1300° C., 1400° C. or any value between 1200-1400° C., and the time may be 1 h, 2 h, 3 h, 4 h, 5 h or any value between 1-5 h.

[0024] Preferably, the amount of the isothiazolinone derivative is 2-3%.

[0025] Optionally, the amount of the isothiazolinone derivative can be 2%, 2.5%, 3% or any value between 2-3%.

[0026] Preferably, the solid content of the slurry is 50-70wt%.

[0027] Optionally, the solid content of the slurry may be 50wt%, 55wt%, 60wt%, 65wt%, 70wt% or any value between 50-70wt%.

[0028] Preferably, the flexible polyurethane foam has a pore size of 10-30 PPI.

[0029] Optionally, the soft polyurethane foam has a pore size of 10PPI, 20PPI, 30PPI or any value between 10-30PPI.

[0030] Preferably, the drying temperature is 20-100°C.

[0031] Optionally, the drying temperature may be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C or any value between 20-100°C.

[0032] Preferably, the first sintering and the second sintering are both performed in an air atmosphere.

[0033] Preferably, the first cooling and the second cooling are natural cooling to room temperature.

[0034] Preferably, the stirring speed is 500-1000 rpm.

[0035] Optionally, the stirring speed may be 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm or any value between 500-1000 rpm.

[0036] Compared with the prior art, the beneficial effects of this application include:

[0037] The present application provides a method for preparing a foam ceramic filter using waste chrome corundum. In order to avoid defects caused by large particles in the preparation of foam ceramics, which affects the filtering effect and service life, the waste chrome corundum is ground and screened in advance, and the small particles under the screen are used; the under the screen is mixed with nano lanthanum oxide, nano cerium oxide, K 4 Sb 2 O 7 Mixed sintering forms complex oxides of chromium, lanthanum, cerium and antimony, solving the problems of chromium pollution and poor filtering effect when using waste chromium corundum; the first powder obtained by sintering is mixed with alumina and zirconium oxide and water to prepare a slurry in the presence of isothiazolinone derivatives and ammonium carbonate as additives, solving the problems of poor compatibility between the first powder and alumina and zirconium oxide, poor structural stability of the filter obtained after sintering, and short service life. DETAILED DESCRIPTION

[0038] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0039] The waste chrome corundum used in the embodiment of the present application is the lining of the waste glass kiln.

[0040] Example 1

[0041] This embodiment provides a method for preparing a foam ceramic filter using waste chromium corundum, which specifically includes the following steps:

[0042] Grinding the waste chrome corundum, and then sieving it with a 200-mesh sieve to obtain the undersize;

[0043] The materials were mixed according to the following ratio: 95% of the sieve material, 2% of nano-lanthanum oxide, 2% of nano-cerium oxide, 0.5% of sodium dodecylbenzene sulfonate, and 0.5% of K 4 Sb 2 O 7 0.5% mixed, first sintered in air atmosphere, then naturally cooled to room temperature, first crushed to obtain first powder; the first sintering temperature is 1100°C, and the time is 6h;

[0044] The materials were mixed according to the following ratio: 70% of the first powder, 20% of aluminum oxide, 5% of zirconium oxide, 1% of the isothiazolinone derivative, and 4% of ammonium carbonate were mixed, water was added, and the mixture was stirred at 500 rpm to prepare a slurry with a solid content of 50 wt%. The structural formula of the isothiazolinone derivative is:

[0045]

[0046] The slurry is impregnated into a soft polyurethane foam having a pore size of 10 PPI as a carrier, and then extruded and dried to obtain a blank;

[0047] The blank is subjected to a second sintering in an air atmosphere and naturally cooled to room temperature to obtain a foam ceramic filter; the second sintering temperature is 1200°C and the time is 5 hours; and the drying temperature is 25°C.

[0048] Example 2

[0049] This embodiment provides a method for preparing a foam ceramic filter using waste chromium corundum, which specifically includes the following steps:

[0050] Grinding the waste chrome corundum, and then sieving it with a 200-mesh sieve to obtain the undersize;

[0051] The materials were mixed according to the following proportions: 97% of the sieve material, 1% of nano-lanthanum oxide, 1% of nano-cerium oxide, 0.9% of sodium dodecylbenzene sulfonate, and 0.5% of K 4 Sb 2 O 7 0.1% mixed, first sintered in air atmosphere, then naturally cooled to room temperature, first crushed to obtain first powder; the first sintering temperature is 1300°C, and the time is 3h;

[0052] The materials were mixed according to the following ratio: 50% of the first powder, 40% of aluminum oxide, 7% of zirconium oxide, 2% of the isothiazolinone derivative, and 1% of ammonium carbonate were mixed, water was added, and the mixture was stirred at 1000 rpm to prepare a slurry with a solid content of 70 wt%. The structural formula of the isothiazolinone derivative is:

[0053]

[0054] The slurry is impregnated into a soft polyurethane foam having a pore size of 20 PPI as a carrier, and then extruded and dried to obtain a blank;

[0055] The blank is subjected to a second sintering in an air atmosphere and naturally cooled to room temperature to obtain a foam ceramic filter; the second sintering temperature is 1400°C and the time is 1 hour; and the drying temperature is 50°C.

[0056] Example 3

[0057] This embodiment provides a method for preparing a foam ceramic filter using waste chromium corundum, which specifically includes the following steps:

[0058] Grinding the waste chrome corundum, and then sieving it with a 200-mesh sieve to obtain the undersize;

[0059] The materials were mixed according to the following ratio: 96% of the sieve material, 1.3% of nano-lanthanum oxide, 1.3% of nano-cerium oxide, 1% of sodium dodecylbenzene sulfonate, and 1% of K 4 Sb 2 O 7 0.4% mixed, first sintered in air atmosphere, then naturally cooled to room temperature, first crushed to obtain first powder; the first sintering temperature is 1200°C, and the time is 5h;

[0060] The materials were mixed according to the following ratio: 55% of the first powder, 25% of aluminum oxide, 10% of zirconium oxide, 5% of the isothiazolinone derivative, and 5% of ammonium carbonate were mixed, water was added, and the mixture was stirred at 800 rpm to prepare a slurry with a solid content of 60 wt%. The structural formula of the isothiazolinone derivative is:

[0061]

[0062] The slurry is impregnated into a soft polyurethane foam having a pore size of 30 PPI as a carrier, and then extruded and dried to obtain a blank;

[0063] The blank is subjected to a second sintering in an air atmosphere and naturally cooled to room temperature to obtain a foam ceramic filter; the second sintering temperature is 1300° C. and the time is 3 hours; and the drying temperature is 100° C.

[0064] Comparative Example 1

[0065] Different from Example 3, the waste chrome corundum is not classified but used directly after grinding.

[0066] Comparative Example 2

[0067] Different from Example 3, the first raw material does not include sodium dodecylbenzene sulfonate.

[0068] Comparative Example 3

[0069] Different from Example 3, the first raw material does not include K 4 Sb 2 O 7 .

[0070] Comparative Example 4

[0071] The difference from Example 3 is that the first raw material does not include sodium dodecylbenzene sulfonate and K 4 Sb 2 O 7 .

[0072] Comparative Example 5

[0073] Different from Example 3, the first raw material does not include nano lanthanum oxide.

[0074] Comparative Example 6

[0075] Different from Example 3, the first raw material does not include nano-cerium oxide.

[0076] Comparative Example 7

[0077] Different from Example 3, the first raw material does not include nano-lanthanum oxide and nano-cerium oxide.

[0078] Comparative Example 8

[0079] Different from Example 3, the second raw material does not include an isothiazolinone derivative.

[0080] Comparative Example 9

[0081] Different from Example 3, the second raw material does not include ammonium carbonate.

[0082] Comparative Example 10

[0083] Different from Example 3, the second raw material does not include isothiazolinone derivatives and ammonium carbonate.

[0084] The foam ceramic filters obtained in the embodiment and the comparative example were prepared into a size of 30*30*20mm, and were tested using aluminum water at a temperature of 700-750°C, with each piece filtering 20kg of aluminum water each time. The aluminum water after one filtration was tested for the detection of chromium, the maximum number of uses (without considering the filtration effect, only observing whether cracks appeared; the data was rounded from the average of multiple tests), the filter opening porosity, and the percentage increase in the tensile strength and elongation of the aluminum water after one filtration. The test results are as follows:

[0085] Table 1 Test results

[0086]

[0087]

[0088] As shown in Table 1 above, the selection of small particle size materials for the classification of waste chrome corundum is helpful to improve the service life and filtering effect; the use of sodium dodecylbenzene sulfonate, K 4 Sb 2 O 7 , nano-lanthanum oxide, and nano-cerium oxide can solve the problems of chromium pollution and poor filtering effect when utilizing waste chromium corundum; the use of isothiazolinone derivatives and ammonium carbonate can solve the problems of poor compatibility between the first powder and alumina and zirconium oxide, poor structural stability of the filter obtained after sintering, and short service life.

[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0090] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for preparing a foam ceramic filter using waste chromium corundum, characterized in that: include: The waste chrome corundum is ground and then sieved with a 200-mesh sieve to obtain the undersize; Mixing first raw materials, performing first sintering, and then performing first cooling and first pulverizing to obtain first powder; The first raw material, calculated with its total mass as 100%, comprises: 95-97% of the sieve undersize, 1-2% of nano lanthanum oxide, 1-2% of nano cerium oxide, 0.5-1% of sodium dodecylbenzene sulfonate, and 0.1-0.5% of K4Sb2O7; The second raw material is mixed, and water is added and stirred to prepare a slurry; the second raw material, calculated based on its own total mass as 100%, includes: 50-70% of the first powder, 20-40% of aluminum oxide, 5-10% of zirconium oxide, 1-5% of isothiazolinone derivative, and 1-5% of ammonium carbonate; the structural formula of the isothiazolinone derivative is: The slurry is impregnated into a soft polyurethane foam as a carrier, and then extruded and dried to obtain a blank; The blank is subjected to a second sintering and a second cooling to obtain a foam ceramic filter.

2. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, characterized in that: The first sintering is performed at a temperature of 1100-1300° C. and for a time of 3-6 hours.

3. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, characterized in that: The second sintering temperature is 1200-1400° C., and the time is 1-5 hours.

4. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, characterized in that: The amount of the isothiazolinone derivative is 2-3%.

5. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, characterized in that: The solid content of the slurry is 50-70 wt %.

6. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, characterized in that: The flexible polyurethane foam has a pore size of 10-30 PPI.

7. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, characterized in that: The drying temperature is 20-100°C.

8. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, characterized in that: The first sintering and the second sintering are both performed in an air atmosphere.

9. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, characterized in that: The first cooling and the second cooling are natural cooling to room temperature.

10. The method according to any one of claims 1 to 9, characterized in that: The stirring speed is 500-1000 rpm.

Citation Information

Patent Citations

  • Ceramic powder composition and slurry, catalyst and carrier as well as preparation method and application

    CN102010184A

  • Weatherproof anti-aging hollow glass sealing gel and preparation method thereof

    CN106336817A

  • Corrosion inhibitor for acid liquor as well as preparation and application of corrosion inhibitor

    CN114437694A

  • Mullite whisker and preparation method thereof

    CN117802584A

  • Composition And Process For Coloring Wood

    US20070131136A1