High-hydrophobicity anti-caking powder and preparation method thereof

Through the preparation of high hydrophobic anti-caking powder, surface modification is used to treat raw materials such as nitrate nitrogen fertilizer and alkyl coupling agent, which solves the problems of nitrate nitrogen fertilizer and moisture absorption, and improves fertilizer fluidity and nutrition Rich effects.

CN118930355APending Publication Date: 2024-11-12ANHUI TIANMO TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410988834.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing anti-caking agents are costly and it is difficult to effectively inhibit the agglomeration and moisture absorption of nitrate nitrogen fertilizers, affecting the storage and transportation of chemical fertilizers.

Method used

Highly hydrophobic anti-caking powder, including nitrate nitrogen fertilizer, alkyl coupling agent, nano-scale silica, organic matter, calcium oxide, ethyl acetate and sodium tert-butoxide, were prepared by surface modification treatment and standstill reaction , an anti-caking agent with high hydrophobicity and trace elements is formed.

Benefits of technology

Effectively inhibit the agglomeration and water absorption of nitrate nitrogen fertilizer, increase particle flow, enrich the nutrients of fertilizers, and improve soil acidity, reduce mutual adhesion between particles, and improve storage and transportation convenience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930355A_ABST
    Figure CN118930355A_ABST
Patent Text Reader

Abstract

The invention discloses high-hydrophobicity anti-caking powder and a preparation method thereof, and relates to the technical field of preparation of anti-caking powder. Comprising the following raw materials in parts by weight: nitrate nitrogen fertilizer, an alkyl coupling agent, nanoscale silicon dioxide, organic matters, calcium oxide, ethyl acetate, ethanol and sodium tert-butoxide. The high-hydrophobicity anti-blocking agent is prepared by carrying out surface coating modification on organic matters by virtue of silane, calcium oxide and nano-scale silicon dioxide and carrying out reaction on the silane and water on the surface under the action of ethyl acetate, ethanol, sodium tert-butoxide and an alkyl coupling agent. The nutrition of the fertilizer is enriched; calcium oxide is easy to form Ca (OH) 2 on the surface of the nitrate nitrogen fertilizer with NH4 < + > in the nitrate nitrogen fertilizer, so that the surfaces of nitrate nitrogen fertilizer particles are effectively isolated from air, the water absorption speed of the particles is reduced, and the purpose of inhibiting the agglomeration of the nitrate nitrogen fertilizer is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anti-caking powder preparation, in particular to a highly hydrophobic anti-caking powder and a preparation method thereof. Background Art

[0002] Fertilizer is an important fertilizer in agricultural production, which can increase crop yields, etc. However, fertilizer is prone to caking during storage, which affects the fertilizer application process and prevents agricultural machinery fertilization. In order to prevent fertilizer from caking, anti-caking agents are generally coated on the surface of fertilizers during the production process to solve the problem of fertilizer caking; fertilizer anti-caking agents are mainly made of fatty acid esters or fatty alcohols, fatty acids, etc. At present, the prices of these raw materials have soared, which has greatly increased the cost of anti-caking agents.

[0003] Anti-caking agent is an additive to promote good fluidity of fertilizers during storage and loading and unloading operations. In order to prevent fertilizer agglomeration, especially the more serious agglomeration of nitrate nitrogen fertilizers, while improving process conditions and controlling particle characteristics, the method of coating nitrate nitrogen fertilizers with anti-caking agents is mainly adopted. The use of anti-caking agent can maximize the inhibition of agglomeration, moisture absorption and pulverization of nitrate nitrogen fertilizers, increase the fluidity of particles, and facilitate the storage, transportation and use of nitrate nitrogen fertilizers. To this end, we proposed a highly hydrophobic anti-caking powder and its preparation method to solve the above problems. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a highly hydrophobic anti-caking powder and a preparation method thereof to solve the problems raised in the above background technology.

[0005] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a highly hydrophobic anti-caking powder, comprising the following raw materials in parts by weight: 40-50 parts of nitrate nitrogen fertilizer, 4-8 parts of alkyl coupling agent, 30-40 parts of nano-silicon dioxide, 20-30 parts of organic matter, 10-15 parts of calcium oxide, 15-18 parts of ethyl acetate, 8-10 parts of ethanol and 10-15 parts of sodium tert-butoxide.

[0006] A method for preparing a highly hydrophobic anti-caking powder comprises the following steps:

[0007] S1. Reserve of raw materials

[0008] Weigh an alkyl coupling agent, ethyl acetate, ethanol, sodium tert-butoxide and calcium oxide in order by weight and set aside;

[0009] S2. Preparation of organic powder

[0010] Using the proportion of calcium oxide to modify the surface of organic matter through a modifying machine to obtain modified organic matter powder;

[0011] S3. Modification treatment

[0012] The organic powder prepared in step S2 is subjected to secondary surface modification by using nano-silicon dioxide in a modifying machine;

[0013] S4, addition of ethyl acetate, ethanol, sodium tert-butoxide

[0014] The modified powder obtained by the secondary modification is cooled to room temperature and then added to a reaction kettle with a stirring device, and the alkyl coupling agent, ethyl acetate, ethanol, and sodium tert-butoxide weighed in step S1 are added to the reaction kettle with a stirring device;

[0015] S5. Static treatment

[0016] The mixture prepared in step S4 is allowed to stand for 8 hours under sealed conditions to obtain the desired highly hydrophobic anti-caking powder.

[0017] To further optimize the technical solution, the alkyl coupling agent is γ-aminopropyltriethoxysilane.

[0018] To further optimize the technical solution, the chemical equation in the process of surface coating modification of organic matter by calcium oxide through a modification machine in step S2 is as follows:

[0019] CaO+NH3·H2O→Ca(OH)2+NH3↑

[0020] To further optimize the technical solution, the chemical equation in the reaction process of ethyl acetate and ethanol in step S4 is as follows:

[0021] CH3COOH+CH3CH2OH→CH3COOCH2CH3+H2O

[0022] To further optimize the technical solution, the anti-caking agent prepared in step S5 is evenly coated on the surface of the nitrate nitrogen fertilizer particles by a screw conveyor.

[0023] To further optimize the technical solution, the organic matter in step S2 is one or a mixture of two or more of the remaining parts of wheat, corn, potato, rapeseed, soybean or sugarcane after harvesting seeds.

[0024] To further optimize the technical solution, the mixture after standing in step S4 is subjected to distillation treatment to remove ethanol and obtain an anti-caking agent.

[0025] To further optimize the technical solution, the anti-caking agent prepared in step S5 is in the form of dry powder, and the anti-caking agent is put into a ball mill and ground to a particle size of 100-200 meshes.

[0026] To further optimize the technical solution, the heating temperature of the reactor of the stirring device in step S4 is 60-70° C., and the stirring time is 50-100 min.

[0027] Beneficial Effects

[0028] Compared with the prior art, the present invention provides a highly hydrophobic anti-caking powder and a preparation method thereof, which has the following beneficial effects:

[0029] 1. The highly hydrophobic anti-caking powder and its preparation method. The calcium oxide and nano-silicon dioxide of the present invention are used to modify the surface of organic matter by coating. Under the action of ethyl acetate, ethanol, sodium tert-butoxide and an alkyl coupling agent, silane reacts with the surface moisture to prepare the required highly hydrophobic anti-caking agent. The anti-caking powder of the present invention solves the agglomeration of nitrate nitrogen fertilizer and at the same time adds trace elements to the fertilizer to enrich the nutrition of the fertilizer.

[0030] 2. The highly hydrophobic anti-caking powder and its preparation method. The anti-caking powder of the present invention utilizes the fact that calcium oxide easily reacts with NH4+ in nitrate nitrogen fertilizer to form Ca(OH)2 on the surface of the fertilizer, thereby effectively isolating the surface of the nitrate nitrogen fertilizer particles from the air, reducing the speed at which the particles absorb water, and reducing the mutual adhesion between particles, thereby inhibiting the agglomeration of nitrate nitrogen fertilizer. At the same time, the preparation of Ca(OH)2 improves the acidity of the soil. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The present invention provides a schematic flow chart of a highly hydrophobic anti-caking powder and a preparation method thereof. DETAILED DESCRIPTION

[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Embodiment 1:

[0034] Please refer to Figure 1 As shown, a highly hydrophobic anti-caking powder comprises the following raw materials in parts by weight: 40-50 parts of nitrate nitrogen fertilizer, 4-8 parts of alkyl coupling agent, 30-40 parts of nano-silicon dioxide, 20-30 parts of organic matter, 10-15 parts of calcium oxide, 15-18 parts of ethyl acetate, 8-10 parts of ethanol and 10-15 parts of sodium tert-butoxide.

[0035] A method for preparing a highly hydrophobic anti-caking powder comprises the following steps:

[0036] S1. Reserve of raw materials

[0037] Weigh an alkyl coupling agent, ethyl acetate, ethanol, sodium tert-butoxide and calcium oxide in order by weight for later use, wherein the alkyl coupling agent is γ-aminopropyltriethoxysilane;

[0038] S2. Preparation of organic powder

[0039] The organic matter is modified by surface coating with calcium oxide in the proportion through a modifier to obtain modified organic powder, wherein the organic matter is one or a mixture of two or more of the remaining parts of wheat, corn, potato, rapeseed, soybean or sugarcane after harvesting seeds; the chemical equation in the surface coating modification reaction process of the organic matter by calcium oxide through the modifier is as follows: CaO+NH3·H2O→Ca(OH)2+NH3↑

[0040] S3. Modification treatment

[0041] The organic powder prepared in step S2 is subjected to secondary surface modification by using nano-silicon dioxide in a modifying machine;

[0042] S4, addition of ethyl acetate, ethanol, sodium tert-butoxide

[0043] The modified powder obtained by the secondary modification is cooled to room temperature and then added to a reactor with a stirring device. The alkyl coupling agent, ethyl acetate, ethanol, and sodium tert-butoxide weighed in step S1 are added to the reactor with a stirring device. The mixture after standing in step S4 is distilled to remove ethanol by distillation to obtain an anti-caking agent; the heating temperature of the reactor of the stirring device is 60-70° C., and the stirring time is 50-100 min; the chemical equation during the reaction of ethyl acetate and ethanol is as follows:

[0044] CH3COOH+CH3CH2OH→CH3COOCH2CH3+H2O;

[0045] S5. Static treatment

[0046] The mixture prepared in step S4 is allowed to stand for 8 hours under sealed conditions to obtain the desired highly hydrophobic anti-caking powder, and the anti-caking agent is evenly coated on the surface of the nitrate nitrogen fertilizer particles by a screw conveyor; the prepared anti-caking agent is in the form of dry powder, and the anti-caking agent is placed in a ball mill and ground to a particle size of 100-200 meshes.

[0047] Embodiment 2:

[0048] Please refer to Figure 1As shown, a highly hydrophobic anti-caking powder comprises the following raw materials in parts by weight: 40-50 parts of nitrate nitrogen fertilizer, 4-8 parts of alkyl coupling agent, 30-40 parts of nano-silicon dioxide, 20-30 parts of organic matter, 10-15 parts of calcium oxide, 15-18 parts of ethyl acetate, 8-10 parts of ethanol and 10-15 parts of sodium tert-butoxide.

[0049] A method for preparing a highly hydrophobic anti-caking powder comprises the following steps:

[0050] S1. Reserve of raw materials

[0051] Weigh an alkyl coupling agent, ethyl acetate, ethanol, sodium tert-butoxide and calcium oxide in order by weight for later use, wherein the alkyl coupling agent is γ-aminopropyltriethoxysilane;

[0052] S2. Preparation of organic powder

[0053] The organic matter is modified by surface coating with calcium oxide in the proportion through a modifier to obtain modified organic powder, wherein the organic matter is one or a mixture of two or more of the remaining parts of wheat, corn, potato, rapeseed, soybean or sugarcane after harvesting seeds; the chemical equation in the surface coating modification reaction process of the organic matter by calcium oxide through the modifier is as follows: CaO+NH3·H2O→Ca(OH)2+NH3↑

[0054] S3. Modification treatment

[0055] The organic powder prepared in step S2 is subjected to secondary surface modification by using nano-silicon dioxide in a modifying machine;

[0056] S4, addition of ethyl acetate, ethanol, sodium tert-butoxide

[0057] The modified powder obtained by the secondary modification is cooled to room temperature and then added to a reactor with a stirring device. The alkyl coupling agent, ethyl acetate, ethanol, and sodium tert-butoxide weighed in step S1 are added to the reactor with a stirring device. The mixture after standing in step S4 is distilled to remove ethanol by distillation to obtain an anti-caking agent; the heating temperature of the reactor of the stirring device is 60-70° C., and the stirring time is 50-100 min; the chemical equation during the reaction of ethyl acetate and ethanol is as follows:

[0058] CH3COOH+CH3CH2OH→CH3COOCH2CH3+H2O;

[0059] S5. Static treatment

[0060] The mixture prepared in step S4 is allowed to stand for 8 hours under sealed conditions to obtain the desired highly hydrophobic anti-caking powder, and the anti-caking agent is evenly coated on the surface of the nitrate nitrogen fertilizer particles by a screw conveyor; the prepared anti-caking agent is in the form of dry powder, and the anti-caking agent is placed in a ball mill and ground to a particle size of 100-200 meshes.

[0061] Embodiment three:

[0062] Please refer to Figure 1 As shown, a highly hydrophobic anti-caking powder comprises the following raw materials in parts by weight: 40-50 parts of nitrate nitrogen fertilizer, 4-8 parts of alkyl coupling agent, 30-40 parts of nano-silicon dioxide, 20-30 parts of organic matter, 10-15 parts of calcium oxide, 15-18 parts of ethyl acetate, 8-10 parts of ethanol and 10-15 parts of sodium tert-butoxide.

[0063] A method for preparing a highly hydrophobic anti-caking powder comprises the following steps:

[0064] S1. Reserve of raw materials

[0065] Weigh an alkyl coupling agent, ethyl acetate, ethanol, sodium tert-butoxide and calcium oxide in order by weight for later use, wherein the alkyl coupling agent is γ-aminopropyltriethoxysilane;

[0066] S2. Preparation of organic powder

[0067] The organic matter is modified by surface coating with calcium oxide in the proportion through a modifier to obtain modified organic powder, wherein the organic matter is one or a mixture of two or more of the remaining parts of wheat, corn, potato, rapeseed, soybean or sugarcane after harvesting seeds; the chemical equation in the surface coating modification reaction process of the organic matter by calcium oxide through the modifier is as follows: CaO+NH3·H2O→Ca(OH)2+NH3↑

[0068] S3. Modification treatment

[0069] The organic powder prepared in step S2 is subjected to secondary surface modification by using nano-silicon dioxide in a modifying machine;

[0070] S4, addition of ethyl acetate, ethanol, sodium tert-butoxide

[0071] The modified powder obtained by the secondary modification is cooled to room temperature and then added to a reactor with a stirring device. The alkyl coupling agent, ethyl acetate, ethanol, and sodium tert-butoxide weighed in step S1 are added to the reactor with a stirring device. The mixture after standing in step S4 is distilled to remove ethanol by distillation to obtain an anti-caking agent; the heating temperature of the reactor of the stirring device is 60-70° C., and the stirring time is 50-100 min; the chemical equation during the reaction of ethyl acetate and ethanol is as follows:

[0072] CH3COOH+CH3CH2OH→CH3COOCH2CH3+H2O;

[0073] S5. Static treatment

[0074] The mixture prepared in step S4 is allowed to stand for 8 hours under sealed conditions to obtain the desired highly hydrophobic anti-caking powder, and the anti-caking agent is evenly coated on the surface of the nitrate nitrogen fertilizer particles by a screw conveyor; the prepared anti-caking agent is in the form of dry powder, and the anti-caking agent is placed in a ball mill and ground to a particle size of 100-200 meshes.

[0075] Experimental Example 4:

[0076] Please refer to Figure 1 As shown, a highly hydrophobic anti-caking powder comprises the following raw materials in parts by weight: 40-50 parts of nitrate nitrogen fertilizer, 4-8 parts of alkyl coupling agent, 30-40 parts of nano-silicon dioxide, 20-30 parts of organic matter, 10-15 parts of calcium oxide, 15-18 parts of ethyl acetate, 8-10 parts of ethanol and 10-15 parts of sodium tert-butoxide.

[0077] A method for preparing a highly hydrophobic anti-caking powder comprises the following steps:

[0078] S1. Reserve of raw materials

[0079] Weigh an alkyl coupling agent, ethyl acetate, ethanol, sodium tert-butoxide and calcium oxide in order by weight for later use, wherein the alkyl coupling agent is γ-aminopropyltriethoxysilane;

[0080] S2. Preparation of organic powder

[0081] The organic matter is modified by surface coating with calcium oxide in the proportion through a modifier to obtain modified organic powder, wherein the organic matter is one or a mixture of two or more of the remaining parts of wheat, corn, potato, rapeseed, soybean or sugarcane after harvesting seeds; the chemical equation in the surface coating modification reaction process of the organic matter by calcium oxide through the modifier is as follows: CaO+NH3·H2O→Ca(OH)2+NH3↑

[0082] S3. Modification treatment

[0083] The organic powder prepared in step S2 is subjected to secondary surface modification by using nano-silicon dioxide in a modifying machine;

[0084] S4, addition of ethyl acetate, ethanol, sodium tert-butoxide

[0085] The modified powder obtained by the secondary modification is cooled to room temperature and then added to a reactor with a stirring device. The alkyl coupling agent, ethyl acetate, ethanol, and sodium tert-butoxide weighed in step S1 are added to the reactor with a stirring device. The mixture after standing in step S4 is distilled to remove ethanol by distillation to obtain an anti-caking agent; the heating temperature of the reactor of the stirring device is 60-70° C., and the stirring time is 50-100 min; the chemical equation during the reaction of ethyl acetate and ethanol is as follows:

[0086] CH3COOH+CH3CH2OH→CH3COOCH2CH3+H2O;

[0087] S5. Static treatment

[0088] The mixture prepared in step S4 is allowed to stand for 8 hours under sealed conditions to obtain the desired highly hydrophobic anti-caking powder, and the anti-caking agent is evenly coated on the surface of the nitrate nitrogen fertilizer particles by a screw conveyor; the prepared anti-caking agent is in the form of dry powder, and the anti-caking agent is placed in a ball mill and ground to a particle size of 100-200 meshes.

[0089] Embodiment five:

[0090] Please refer to Figure 1 As shown, a highly hydrophobic anti-caking powder comprises the following raw materials in parts by weight: 40-50 parts of nitrate nitrogen fertilizer, 4-8 parts of alkyl coupling agent, 30-40 parts of nano-silicon dioxide, 20-30 parts of organic matter, 10-15 parts of calcium oxide, 15-18 parts of ethyl acetate, 8-10 parts of ethanol and 10-15 parts of sodium tert-butoxide.

[0091] A method for preparing a highly hydrophobic anti-caking powder comprises the following steps:

[0092] S1. Reserve of raw materials

[0093] Weigh an alkyl coupling agent, ethyl acetate, ethanol, sodium tert-butoxide and calcium oxide in order by weight for later use, wherein the alkyl coupling agent is γ-aminopropyltriethoxysilane;

[0094] S2. Preparation of organic powder

[0095] The organic matter is modified by surface coating with calcium oxide in the proportion through a modifier to obtain modified organic powder, wherein the organic matter is one or a mixture of two or more of the remaining parts of wheat, corn, potato, rapeseed, soybean or sugarcane after harvesting seeds; the chemical equation in the surface coating modification reaction process of the organic matter by calcium oxide through the modifier is as follows: CaO+NH3·H2O→Ca(OH)2+NH3↑

[0096] S3. Modification treatment

[0097] The organic powder prepared in step S2 is subjected to secondary surface modification by using nano-silicon dioxide in a modifying machine;

[0098] S4, addition of ethyl acetate, ethanol, sodium tert-butoxide

[0099] The modified powder obtained by the secondary modification is cooled to room temperature and then added to a reactor with a stirring device. The alkyl coupling agent, ethyl acetate, ethanol, and sodium tert-butoxide weighed in step S1 are added to the reactor with a stirring device. The mixture after standing in step S4 is distilled to remove ethanol by distillation to obtain an anti-caking agent; the heating temperature of the reactor of the stirring device is 60-70° C., and the stirring time is 50-100 min; the chemical equation during the reaction of ethyl acetate and ethanol is as follows:

[0100] CH3COOH+CH3CH2OH→CH3COOCH2CH3+H2O;

[0101] S5. Static treatment

[0102] The mixture prepared in step S4 is allowed to stand for 8 hours under sealed conditions to obtain the desired highly hydrophobic anti-caking powder, and the anti-caking agent is evenly coated on the surface of the nitrate nitrogen fertilizer particles by a screw conveyor; the prepared anti-caking agent is in the form of dry powder, and the anti-caking agent is placed in a ball mill and ground to a particle size of 100-200 meshes.

[0103] Judging criteria:

[0104] Table 1 is a comparison of the caking rate % data of Examples 1 to 5 and the control group (commercially available) at different times (h) under the same temperature (°C) and humidity, as shown in Table 1 below:

[0105]

[0106] Table 2 shows the caking rate data of the highly hydrophobic anti-caking powder prepared in Examples 1 to 5 after being added to nitrate nitrogen fertilizer at the same time, as shown in Table 2 below:

[0107]

[0108] It can be seen from Tables 1-2 that the highly hydrophobic anti-caking powder prepared by the present invention has broad application prospects. By comparing the five embodiments, the best effect is embodiment 1. Therefore, embodiment 1 is selected as the best embodiment. Specific changes in the amount also fall within the scope of protection of this technical solution.

[0109] The beneficial effects of the invention are as follows: the highly hydrophobic anti-caking powder and its preparation method, the calcium oxide and nano-silicon dioxide of the invention carry out surface coating modification on organic matter, under the action of ethyl acetate, ethanol, sodium tert-butoxide and an alkyl coupling agent, silane reacts with surface moisture to prepare the required highly hydrophobic anti-caking agent, the anti-caking agent of the invention solves the agglomeration of nitrate nitrogen fertilizer, and at the same time, trace elements are added to the fertilizer to enrich the nutrition of the fertilizer; the anti-caking agent of the invention utilizes the fact that calcium oxide easily reacts with NH4+ in the nitrate nitrogen fertilizer to form Ca(OH)2 on the surface of the fertilizer, so that the surface of the nitrate nitrogen fertilizer particles is effectively isolated from the air, the speed at which the particles absorb water is reduced, and the mutual adhesion between the particles is reduced, so as to inhibit the agglomeration of the nitrate nitrogen fertilizer, and at the same time, the preparation of Ca(OH)2 improves the acidity of the soil.

[0110] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A highly hydrophobic anti-caking powder, characterized in that: The invention comprises the following raw materials in parts by weight: 40-50 parts of nitrate nitrogen fertilizer, 4-8 parts of alkyl coupling agent, 30-40 parts of nano-silicon dioxide, 20-30 parts of organic matter, 10-15 parts of calcium oxide, 15-18 parts of ethyl acetate, 8-10 parts of ethanol and 10-15 parts of sodium tert-butoxide.

2. A highly hydrophobic anti-caking powder according to claim 1, characterized in that: The alkyl coupling agent is γ-aminopropyltriethoxysilane.

3. A method for preparing a highly hydrophobic anti-caking powder according to claim 1-2, characterized in that: The following steps are involved: S1. Reserve of raw materials Weigh an alkyl coupling agent, ethyl acetate, ethanol, sodium tert-butoxide and calcium oxide in order by weight and set aside; S2. Preparation of organic powder Using the proportion of calcium oxide to modify the surface of organic matter through a modifying machine to obtain modified organic matter powder; S3. Modification treatment The organic powder prepared in step S2 is subjected to secondary surface modification by using nano-silicon dioxide in a modifying machine; S4, addition of ethyl acetate, ethanol, sodium tert-butoxide The modified powder obtained by the secondary modification is cooled to room temperature and then added to a reaction kettle with a stirring device, and the alkyl coupling agent, ethyl acetate, ethanol, and sodium tert-butoxide weighed in step S1 are added to the reaction kettle with a stirring device; S5. Static treatment The mixture prepared in step S4 is allowed to stand for 8 hours under sealed conditions to obtain the desired highly hydrophobic anti-caking powder.

4. A method for preparing a highly hydrophobic anti-caking powder according to claims 1-3, characterized in that: The chemical equation in the process of surface coating modification reaction of organic matter by calcium oxide through the modification machine in step S2 is as follows: CaO+NH3·H2O→Ca(OH)2+NH3↑ 5. A method for preparing a highly hydrophobic anti-caking powder according to claims 1-3, characterized in that: The chemical equation in the reaction process of ethyl acetate and ethanol in step S4 is as follows: CH3COOH+CH3CH2OH→CH3COOCH2CH3+H2O 6. A method for preparing a highly hydrophobic anti-caking powder according to claims 1-3, characterized in that: The anti-caking agent prepared in step S5 is evenly coated on the surface of the nitrate nitrogen fertilizer particles by a screw conveyor.

7. A method for preparing a highly hydrophobic anti-caking powder according to claims 1-3, characterized in that: The organic matter in step S2 is one or a mixture of two or more of the remaining parts of wheat, corn, potato, rapeseed, soybean or sugarcane after harvesting seeds.

8. A method for preparing a highly hydrophobic anti-caking powder according to claims 1-3, characterized in that: The mixture after standing in step S4 is subjected to distillation treatment to remove ethanol and obtain an anti-caking agent.

9. A method for preparing a highly hydrophobic anti-caking powder according to claims 1-3, characterized in that: The anti-caking agent prepared in step S5 is in the form of dry powder. The prepared anti-caking agent is put into a ball mill and ground to a particle size of 100-200 meshes to obtain a highly hydrophobic anti-caking powder.

10. A method for preparing a highly hydrophobic anti-caking powder according to claims 1-3, characterized in that: The heating temperature of the reactor of the stirring device in step S4 is 60-70° C., and the stirring time is 50-100 min.

Citation Information

Cited By

  • Anti-blocking agent for potassium chloride particles as well as preparation method and application of anti-blocking agent