Organic film forming material, pattern forming method, and compound for organic film

By using organic film forming materials with specific aromatic ring substituents and multilayer photoresist treatment, the problems of reduced resolution and poor etching selectivity of photoresist films were solved, enabling the formation of high-precision micro-patterns and the planarization of substrates, thus meeting the processing requirements of complex substrate structures.

CN118930452APending Publication Date: 2024-11-12SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410567598.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing technology, with the high integration and high speed of LSI, the resolution performance of photoresist film is reduced, the pattern collapse and the etching selectivity are poor, which makes it impossible for the resist pattern to be correctly transferred to the substrate being processed. In addition, the planarization and embedding characteristics of the lower resist film in the multilayer resist method are insufficient, making it difficult to meet the processing requirements of complex substrate structures.

Method used

Organic film forming materials containing specific aromatic ring substituents are used. Through 3 or 4 layers of photoresist treatment, a multi-layer photoresist structure is formed by using a silicon-containing photoresist intermediate film and an organic anti-reflective film. Combined with photolithography technology, high-precision pattern transfer and substrate planarization are achieved.

Benefits of technology

It enables the formation of high-precision, fine patterns on complex substrate structures, improves etching resistance and planarization characteristics, and ensures the correct transfer of resist patterns and substrate processing quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930452A_ABST
    Figure CN118930452A_ABST
Patent Text Reader

Abstract

The invention relates to an organic film forming material, a pattern forming method, and a compound for an organic film. The present invention provides a compound for an organic film, which is capable of forming an organic film having excellent heat resistance, excellent embedding and planarization properties of a pattern formed on a substrate, and good film-forming properties and adhesion to the substrate, and provides an organic film-forming material containing the compound, and a pattern-forming method using the material. An organic film-forming material characterized by containing a compound for an organic film represented by general formula (1) and an organic solvent. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an organic film forming material, a pattern forming method, and a compound for an organic film. Background Art

[0002] With the high integration and high speed of LSI, the miniaturization of pattern size is progressing rapidly. In response to this miniaturization, photolithography technology has achieved the formation of fine patterns by shortening the wavelength of the light source and appropriately selecting the corresponding resist composition. The core of this is the positive photoresist composition used in a single layer. This single-layer positive photoresist composition has a skeleton in the resist resin that is etch-resistant to dry etching using chlorine-based or fluorine-based gas plasma, and has a switching mechanism that allows the exposed part to dissolve, so that the exposed part is dissolved and a pattern is formed, and the substrate to be processed is dry-etched using the remaining resist pattern as an etching mask.

[0003] However, if the thickness of the photoresist film used is directly miniaturized, that is, if the pattern width is reduced, the resolution performance of the photoresist film will be reduced, and if the photoresist film is to be patterned using a developer, the so-called aspect ratio will become too large, resulting in problems such as pattern collapse. Therefore, as the pattern is miniaturized, the photoresist film will become thinner and thinner.

[0004] On the other hand, the processing of the processed substrate usually uses a method of processing the substrate by dry etching using a photoresist film with a pattern as an etching mask, but in reality there is no dry etching method that can obtain complete etching selectivity between the photoresist film and the processed substrate. Therefore, during the substrate processing, even the resist film will be damaged and collapsed, and there will be problems such as the inability to correctly transfer the resist pattern to the processed substrate. Therefore, with the miniaturization of the pattern, the resist composition is required to have higher dry etching resistance. But on the other hand, in order to improve the resolution, the resin used in the photoresist composition needs to be a resin with low light absorption at the exposure wavelength. Therefore, as the exposure light wavelength shortens to i-rays, KrF, and ArF, the resin also changes to novolac resin, polyhydroxystyrene, and resins with aliphatic polycyclic skeletons. However, in reality, under the dry etching conditions during substrate processing, the etching speed becomes faster, and the recent photoresist composition with high resolution tends to weaken the etching resistance.

[0005] Therefore, it is necessary to perform dry etching processing on the substrate to be processed using a thinner photoresist film with weaker etching resistance, and it is important to ensure the material and treatment in this processing step.

[0006] As one of the methods to solve such a problem, there is a multilayer resist method. In this method, a resist lower film having a different etching selectivity from the photoresist film (i.e., the resist upper film) is inserted between the resist upper film and the substrate to be processed, and after the resist upper film has a pattern, the resist upper film pattern is used as a dry etching mask to transfer the pattern to the resist lower film by dry etching, and then the resist lower film is used as a dry etching mask to transfer the pattern to the substrate to be processed by dry etching.

[0007] As one of the multilayer resist methods, there is a three-layer resist method that can be performed using a general resist composition used in the single-layer resist method. This three-layer resist method, for example, forms an organic film made of novolac resin or the like as a resist lower film on a substrate to be processed, forms a silicon-containing film thereon as a resist intermediate film, and forms a normal organic photoresist film thereon as a resist upper film. When dry etching is performed using fluorine-based gas plasma, the organic resist upper film can achieve a good etching selectivity ratio with respect to the silicon-containing resist intermediate film, so the resist upper film pattern can be transferred to the silicon-containing resist intermediate film by dry etching using fluorine-based gas plasma. According to this method, even if a resist composition that is difficult to form a pattern having a sufficient film thickness for directly processing a substrate to be processed or a resist composition that does not have sufficient dry etching resistance for substrate processing is used, a pattern can be transferred to a silicon-containing resist intermediate film, and if the pattern transfer is subsequently performed by dry etching using oxygen or hydrogen gas plasma, a pattern of an organic film (resist underlayer film) made of a novolac resin or the like having sufficient dry etching resistance for substrate processing can be obtained. Many resist underlayer films such as the above-mentioned resist underlayer films, such as the resist underlayer films described in Patent Document 1, are already known.

[0008] On the other hand, in recent years, there have been active studies on the manufacture of semiconductor devices with new structures such as multi-gate structures, and in response to this, better and superior planarization and filling characteristics are required for the resist lower film. For example, when the base substrate to be processed has micro-pattern structures such as holes, trenches, and fins, it is necessary to utilize the resist lower film to fill the pattern with a film without gaps (gap-filling) characteristics. In addition, when there is a height difference in the base substrate to be processed, and when there are pattern-dense parts and pattern-free areas on the same wafer, it is necessary to planarize the film surface with the resist lower film. By planarizing the surface of the resist lower film, the film thickness variation of the resist intermediate film and the resist upper film formed thereon can be suppressed, and the focus tolerance of the lithography and the tolerance reduction in the subsequent processing steps of the processed substrate can be suppressed.

[0009] Furthermore, organic film materials with excellent filling / planarization characteristics are not limited to underlayer films for multilayer resists, but can also be widely used as planarization materials for semiconductor device manufacturing, such as planarization of substrates before patterning using nanostamping. Furthermore, overall planarization in the semiconductor device manufacturing process is currently generally performed using CMP processing, but CMP is a high-cost process, and there is also a desire for materials that can serve as an alternative overall planarization method.

[0010] In order to form a planarization film for planarizing a semiconductor substrate with uneven surfaces, a resist underlayer film material containing a polymer obtained by reacting an aromatic compound with a compound having a carbonyl group or other carbon-oxygen double bond has been proposed (Patent Document 2). However, the planarization performance of the aforementioned material in a wide trench portion of a substrate is not satisfactory in response to the requirements of the most advanced devices, and a resist underlayer film material with excellent planarity on a wider substrate structure is sought.

[0011] As mentioned above, the structure of the processed substrate has become more complicated, and some people have also studied the use of novel materials with high electron mobility such as strained silicon and gallium arsenide on the surface of the processed substrate, and ultra-thin film polysilicon controlled in angstrom units, etc. It is speculated that films can be formed on a variety of processed substrate surface shapes and materials. Therefore, in order to ensure the processing tolerance, not only excellent flattening characteristics, but also the ability to form films independently of the material and shape of the processed substrate has become an important characteristic.

[0012] Prior art literature

[0013] Patent Literature

[0014] [Patent Document 1] Japanese Patent Application Publication No. 2004-205685

[0015] [Patent Document 2] International Publication No. 2019 / 225615 Summary of the invention

[0016] [Problems to be solved by the invention]

[0017] In view of the above situation, the present invention aims to provide an organic film compound that can form an organic film that has not only excellent heat resistance, filling and planarization characteristics of the pattern formed on the substrate, but also good film forming properties and adhesion to the substrate, an organic film forming material containing the above-mentioned compound, and a pattern forming method using the above-mentioned material.

[0018] [Methods for solving problems]

[0019] In order to solve the above-mentioned problems, the present invention provides an organic film-forming material comprising an organic film-forming compound represented by the following general formula (1) and an organic solvent.

[0020] [Chemistry 1]

[0021]

[0022] Where W 1 For n containing aromatic rings 1 valent organic group, L is a substituent on the aromatic ring and is represented by the following general formula (2): 1 , L 2 or both. Let the total number of substituents L on the aromatic ring be n 1 , L 1 The number of x, L 2 When the number of is y, it satisfies x+y=n 1 , 2≤n 1 The relationship is ≤8, 0≤y≤8, 0≤x≤8.

[0023] [Chemistry 2]

[0024]

[0025] Where n 2 represents an integer from 1 to 3, R 1 is any of the following formula (3), R 2 It is any one of the following general formula (4).

[0026] [Chemistry 3]

[0027]

[0028] [Chemistry 4]

[0029]

[0030] In the formula, R 3 is any of the following formula (5), n 3 Indicates 0 or 1, n 4 Indicates 1 or 2.

[0031] [Chemistry 5]

[0032]

[0033] Such an organic film forming material can form an organic film which is excellent in heat resistance, filling and planarization properties of a pattern formed on a substrate, and has good film-forming properties and adhesion to the substrate.

[0034] In the present invention, L constituting the substituent L on the aromatic ring of the organic film compound represented by the general formula (1) is 1 , L 2 Those represented by the following general formula (6) are preferred.

[0035] [Chemistry 6]

[0036]

[0037] In the formula, R 1 and R 2 Same as above.

[0038] By introducing such a structure, it is possible to achieve both the contradictory characteristics of thermal fluidity and heat resistance.

[0039] In the present invention, L constituting the substituent L on the aromatic ring of the organic film compound represented by the general formula (1) is 1 , L 2 R 1 , R 2 , any of the combinations represented by the following general formula (7) is preferred.

[0040] [Chemistry 7]

[0041]

[0042] In the formula, R 3 、n 4 Same as above.

[0043] By configuring in such a combination, the heat curing property can be improved, and an organic film having excellent heat resistance can be formed.

[0044] The total number n of substituents L on the aromatic ring of the organic film compound represented by the general formula (1) is 1 , preferably 3≤n 1 ≤6 is better.

[0045] By adjusting the number of thermosetting groups as the substitution group within such a range, the number of thermosetting groups will not be excessive, so that drastic thermosetting will not occur and the thermal fluidity will not be reduced. Therefore, there is no risk of deterioration of planarization characteristics or insufficient solvent resistance and heat resistance due to insufficient thermosetting groups.

[0046] In the present invention, the ratio Mw / Mn of the polystyrene-equivalent weight average molecular weight Mw and the number average molecular weight Mn of the organic membrane compound obtained by gel permeation chromatography is preferably 1.00≤Mw / Mn≤1.15.

[0047] With such Mw / Mn, an organic film having excellent filling characteristics and flatness can be formed.

[0048] In the present invention, the organic solvent is preferably a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.

[0049] When the organic solvent is the mixture, the addition of the high-boiling-point solvent to the organic film-forming compound provides thermal fluidity to the organic film, and the organic film-forming material has both high filling and planarizing properties.

[0050] Furthermore, in the present invention, it is preferred that the organic film-forming material further contains one or more of a surfactant and a plasticizer.

[0051] An organic film forming material containing such a component has better coating properties and filling / planarization characteristics.

[0052] The present invention also provides a pattern forming method, which is a method for forming a pattern on a workpiece, comprising forming an organic film on the workpiece using the organic film forming material described above.

[0053] On the organic film, a silicon-containing resist intermediate film is formed using a silicon-containing resist intermediate film material.

[0054] A photoresist composition is used to form a resist upper film on the silicon-containing resist intermediate film.

[0055] forming a circuit pattern on the resist upper film,

[0056] The pattern is transferred to the silicon-containing resist intermediate film by etching using the patterned resist upper film as a mask.

[0057] The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film having the transferred pattern as a mask.

[0058] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0059] The pattern forming method using the three-layer resist process can form a fine pattern with high precision on a workpiece.

[0060] The present invention also provides a pattern forming method, which is a method for forming a pattern on a workpiece, wherein an organic film is formed on the workpiece using the organic film forming material described above.

[0061] On the organic film, a silicon-containing resist intermediate film is formed using a silicon-containing resist intermediate film material.

[0062] forming an organic anti-reflective film (BARC) on the aforementioned silicon-containing resist intermediate film,

[0063] On the aforementioned BARC, a resist upper layer film is formed using a photoresist composition to form a 4-layer film structure.

[0064] forming a circuit pattern on the resist upper film,

[0065] The aforementioned patterned resist upper layer film is used as a mask, and the aforementioned BARC is transferred to the aforementioned silicon-containing resist intermediate film by etching.

[0066] The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film having the transferred pattern as a mask.

[0067] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0068] The pattern forming method using the four-layer resist process can form a fine pattern on a workpiece with higher precision.

[0069] The present invention also provides a pattern forming method, which is a method for forming a pattern on a workpiece, comprising forming an organic film on the workpiece using the organic film forming material described above.

[0070] On the organic film, an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film is formed.

[0071] On the inorganic hard mask intermediate film, a resist upper layer film is formed using a photoresist composition.

[0072] forming a circuit pattern on the resist upper film,

[0073] The pattern is transferred to the inorganic hard mask intermediate film by etching using the patterned resist upper film as a mask.

[0074] The inorganic hard mask intermediate film with the transferred pattern is used as a mask to transfer the pattern to the organic film by etching.

[0075] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0076] The pattern forming method using the three-layer resist process can form a fine pattern on a workpiece with high precision.

[0077] The present invention also provides a pattern forming method, which is a method for forming a pattern on a workpiece, comprising forming an organic film on the workpiece using the organic film forming material described above.

[0078] On the aforementioned organic film, an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film is formed;

[0079] On the inorganic hard mask intermediate film, an organic anti-reflection film (BARC) is formed.

[0080] On the aforementioned BARC, a resist upper layer film is formed using a photoresist composition to form a 4-layer film structure.

[0081] forming a circuit pattern on the resist upper film,

[0082] The patterned resist upper film is used as a mask, and the BARC is etched to transfer the pattern to the inorganic hard mask intermediate film.

[0083] The inorganic hard mask intermediate film with the transferred pattern is used as a mask to transfer the pattern to the organic film by etching.

[0084] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0085] The pattern forming method using the four-layer resist process can form a fine pattern on a workpiece with higher precision.

[0086] In this case, the inorganic hard mask intermediate film is preferably formed by a CVD method or an ALD method.

[0087] When the inorganic hard mask intermediate film is formed by the CVD method or the ALD method, a fine pattern can be formed on the workpiece with higher precision.

[0088] At this time, the patterning method of the resist upper layer film is preferably a patterning method using optical lithography with a wavelength of 10 nm to 300 nm, direct writing using an electron beam, nanoimprinting, or a combination thereof.

[0089] The method for forming a circuit on the resist upper layer film mentioned above can form a fine pattern on the workpiece with higher precision by using the above method.

[0090] At this time, the development method of the above-mentioned pattern forming method is preferably alkali development or organic solvent development.

[0091] When alkali development or organic solvent development is used as the development method, a fine pattern can be formed on the workpiece with higher precision.

[0092] At this time, the aforementioned processed body is preferably a semiconductor device substrate, or a semiconductor device substrate on which any of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film is formed.

[0093] In the present invention, for example, the above-mentioned object to be processed can be used.

[0094] At this time, the aforementioned metal is preferably silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, manganese, molybdenum, ruthenium or an alloy thereof.

[0095] As the above-mentioned metals, any of these can be used.

[0096] The present invention also provides a compound for an organic film represented by the following general formula (1).

[0097] [Chemistry 8]

[0098]

[0099] Where W 1 For n containing aromatic rings 1 valent organic group, L is a substituent on the aromatic ring and is represented by the following general formula (2): 1 , L 2 or both. Let the total number of substituents L on the aromatic ring be n 1 , L 1 The number of x, L 2 When the number of is y, it satisfies x+y=n 1 , 2≤n 1 The relationship is ≤8, 0≤y≤8, 0≤x≤8.

[0100] [Chemistry 9]

[0101]

[0102] Where n 2 represents an integer from 1 to 3, R 1 is any of the following formula (3), R 2 It is any one of the following general formula (4).

[0103] [Chemistry 10]

[0104]

[0105] [Chemistry 11]

[0106]

[0107] In the formula, R 3 is any of the following formula (5), n 3 Indicates 0 or 1, n 4 Indicates 1 or 2.

[0108] [Chemistry 12]

[0109]

[0110] Such a compound for an organic film can be used as an organic film-forming material capable of forming an organic film having excellent heat resistance, filling and planarizing properties of a pattern formed on a substrate, and good film-forming properties and adhesion to a substrate.

[0111] [Effects of the Invention]

[0112] As described above, the organic film forming material of the present invention is a useful material for forming an organic film that has various properties such as heat resistance and filling / planarization properties and can be formed without dependence on the processed substrate. Therefore, it is very useful as an organic film forming material in multilayer resist processes such as two-layer resist process, three-layer resist process using a silicon-containing resist underlayer film, or four-layer resist process using a silicon-containing resist intermediate film and an organic antireflection film, or a planarization material for semiconductor device manufacturing. In addition, in the pattern forming method of the present invention, a fine pattern can be formed on a processed substrate with high precision in a multilayer resist process.

[0113] The organic film compound of the present invention represented by the above general formula (1) has excellent heat resistance and thermal curing properties, and can be used as an organic film material as a compound monomer. Due to its excellent thermal fluidity, when the organic film is used as an anti-etching underlayer film, it also has excellent filling / planarization properties for the pattern substrate.

[0114] In addition, since the molecule has an amide structure, not only heat resistance but also adhesion to the substrate and film forming properties are improved. In addition, by introducing an alkylene group between the amide structure and the aromatic ring to reduce crystallinity, not only thermal fluidity but also film forming properties are improved. Furthermore, by appropriately selecting W 1 By indicating the main skeleton, various physical properties such as optical characteristics and etching resistance when the organic film is used as a resist underlayer film can be adjusted according to the required performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0115] Figure 1 (A) to (F) are explanatory diagrams of an example of a pattern forming method using a three-layer resist process of the present invention.

[0116] Figure 2 (G) to (I) are explanatory diagrams of the landfill characteristic evaluation method of the embodiment.

[0117] Figure 3 (J) and (K) are explanatory diagrams of the planarization characteristic evaluation method of the embodiment.

[0118] Figure 4 It is an explanatory diagram of the adhesion measurement method of the Example. DETAILED DESCRIPTION

[0119] As mentioned above, an organic film forming material, a pattern forming method using the same, and a compound for an organic film are sought that can form an organic film with excellent film-forming properties and flatness even on a processed substrate having a portion that is particularly difficult to flatten, such as a wide trench structure, in a fine patterning process using a multilayer resist method in a semiconductor device manufacturing step.

[0120] The inventors of the present application have found that an organic film forming material using a specific compound having a substituent on an aromatic ring of the present invention is useful for forming an organic film having excellent filling / planarization characteristics, and have completed the present invention.

[0121] That is, the present invention is an organic film-forming material comprising an organic film-forming compound represented by the following general formula (1) and an organic solvent.

[0122] [Chemistry 13]

[0123]

[0124] Where W 1 For n containing aromatic rings 1 valent organic group, L is a substituent on the aromatic ring and is represented by the following general formula (2): 1 , L 2 or both. Let the total number of substituents L on the aromatic ring be n 1 , L 1 The number of x, L 2 When the number of is y, it satisfies x+y=n 1 , 2≤n 1 The relationship is ≤8, 0≤y≤8, 0≤x≤8.

[0125] [Chemistry 14]

[0126]

[0127] Where n 2 represents an integer from 1 to 3, R 1 is any of the following formula (3), R 2 It is any one of the following general formula (4).

[0128] [Chemistry 15]

[0129]

[0130] [Chemistry 16]

[0131]

[0132] In the formula, R 3 is any of the following formula (5), n 3Indicates 0 or 1n 4 Indicates 1 or 2.

[0133] [Chemistry 17]

[0134]

[0135] The present invention is described in detail below, but the present invention is not limited thereto.

[0136] <Organic film forming material>

[0137] The organic film-forming material of the present invention contains a compound for an organic film represented by the following general formula (1) and an organic solvent. Each component contained in the organic film-forming material of the present invention will be described in detail below.

[0138] <Compounds for organic membranes>

[0139] The compound for organic film of the present invention is represented by the following general formula (1).

[0140] [Chemistry 18]

[0141]

[0142] Where W 1 For n containing aromatic rings 1 valent organic group, L is a substituent on the aromatic ring and is represented by the following general formula (2): 1 , L 2 or both. Let the total number of substituents L on the aromatic ring be n 1 , L 1 The number of x, L 2 When the number of is y, it satisfies x+y=n 1 , 2≤n 1 The relationship is ≤8, 0≤y≤8, 0≤x≤8.

[0143] [Chemistry 19]

[0144]

[0145] Where n 2 represents an integer from 1 to 3, R 1 is any of the following formula (3), R 2 It is any one of the following general formula (4).

[0146] [Chemistry 20]

[0147]

[0148] [Chemistry 21]

[0149]

[0150] In the formula, R 3 is any of the following formula (5), n 3 Indicates 0 or 1n 4 Indicates 1 or 2.

[0151] [Chemistry 22]

[0152]

[0153] In the above general formula (1), W 1 For n containing aromatic rings 1 The valent organic group, specifically, for example, the structure shown below. These aromatic rings may also have substitutions other than L, such as alkyl groups with 1 to 10 carbon atoms, alkynyl or alkenyl groups with 3 to 10 carbon atoms, aryl groups with 6 to 10 carbon atoms, nitro groups, halogen groups, nitrile groups, sulfonyl groups, alkoxycarbonyl groups with 2 to 10 carbon atoms, alkanoyloxy groups with 2 to 10 carbon atoms, etc.

[0154] [Chemistry 23]

[0155]

[0156] [Chemistry 24]

[0157]

[0158] [Chemistry 25]

[0159]

[0160] [Chemistry 26]

[0161]

[0162] [Chemistry 27]

[0163]

[0164] [Chemistry 28]

[0165]

[0166] [Chemistry 29]

[0167]

[0168] [Chemistry 30]

[0169]

[0170] [Chemistry 31]

[0171]

[0172] [Chemistry 32]

[0173]

[0174] The total number n of substituents L on the aromatic ring of the organic film compound represented by the general formula (1) is 1 , which satisfies 3≤n 1 ≤6 is better.

[0175] Again, W 1 The structural formula of the above general formula (1) represented by L is preferably the structural formula represented by the following general formula (8), that is, the substituent L on the aromatic ring is substituted by the following W 2 And the substituent of the aromatic ring bonded by ether bond is preferred. 2 n 6 valent organic group, n 5 Indicates 1 or 2, n 6 represents an integer of 1 to 3. In this case, the number of substituents L on the aromatic ring in the general formula (1) is n 1 Become 5 With n 6 The product of, at this time, meets 3≤n 5 ×n 6 ≤6. In this way, and W 2 By using a substituent on an aromatic ring via an ether bond as a connecting group, thermal fluidity can be imparted without impairing heat resistance.

[0176] [Chemistry 33]

[0177]

[0178] W in the above general formula (8) 2 Such a structure is more ideal from the perspective of easy access to raw materials.

[0179] [Chemistry 34]

[0180]

[0181] In the formula, the chain line represents the atomic bond.

[0182] The substituent L on the aromatic ring represented by the general formula (2) is L 1 or L 2 In the formula, the substitution is carried out by an oxygen atom or a nitrogen atom containing R 1 , R 2 The structure of the substituent is L 1 The oxygen atoms below and L 2 The nitrogen atom and the like are the same. If the terminal group structure of the same structure is simply represented by R 4 Indicates that L 1 , L2 It can be represented by the following general formula (9).

[0183] [Chemistry 35]

[0184]

[0185] In the formula, R 1 , R 2 、n 2 Same as above.

[0186] In the above general formula (9), L 1 and L 2 R 4 , the following structures can be listed. 4 The alkylene chain connecting the atomic bond and the amide bond in the film is a linking group that helps impart fluidity and film-forming properties. By combining with the hardening properties of the cross-linking group with an unsaturated bond at the end, it will exhibit flatness and fluidity. By introducing the alkylene chain, even if W 1 When the skeleton is a rigid structure, it can still relax the crystallinity and give thermal fluidity and film-forming properties. 2 = 1 and having a propargyl group or an ethynyl group is more preferred from the viewpoint of heat resistance. 1 Not a hydrogen atom, that is, R 1 , R 2 Those having a tertiary amide structure having a substituent other than a hydrogen atom are more preferred from the viewpoint of imparting thermal fluidity and improving solvent solubility (in the following formula, n 2 As before, the chains represent atomic bonds with oxygen and nitrogen atoms.)

[0187] [Chemistry 36]

[0188]

[0189] [Chemistry 37]

[0190]

[0191] [Chemistry 38]

[0192]

[0193] L constituting the substituent L on the aromatic ring of the organic film compound represented by the general formula (1) 1 , L 2 , preferably represented by the following general formula (6). From the viewpoint of the synthesis of the compound and the heat resistance of the obtained compound, the following examples are preferred.

[0194] [Chemistry 39]

[0195]

[0196] In the formula, R 1 and R 2 Same as above.

[0197] L constituting the substituent L on the aromatic ring of the organic film compound represented by the general formula (1) 1 , L 2 R 1 , R 2 , preferably any one of the combinations represented by the following general formula (7). By such a combination, an organic film having a good balance between thermosetting property and thermal fluidity and excellent heat resistance can be formed.

[0198] [Chemistry 40]

[0199]

[0200] In the formula, R 3 、n 4 Same as above.

[0201] Furthermore, L constituting the substituent L of the aromatic ring 1 , L 2 The substituent R 1 , R 2 Specifically, as described in the production method, multiple reagents for introducing terminal groups can be used in combination to adjust L in any ratio. 1 , L 2 The substituent R 1 , R 2 proportion.

[0202] In addition, the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the organic membrane compound represented by the above general formula (1) obtained by gel permeation chromatography in terms of polystyrene is preferably 1.00≤Mw / Mn≤1.15, and more preferably 1.00≤Mw / Mn≤1.10. By definition, if it is a monomolecular compound, Mw / Mn will be 1.00, but due to the separation properties of gel permeation chromatography, the measured value may exceed 1.00. In general, if a polymer having repeating units does not use a special polymerization method, it is extremely difficult to approach Mw / Mn=1.00, and it will have a distribution of Mw and Mw / Mn will become a value exceeding 1. In the present invention, in order to distinguish monomolecular compounds from polymers, 1.00≤Mw / Mn≤1.15 is defined as an index representing monomolecularity. When a compound composed of multiple terminal group structures is used, the Mw / Mn distribution of a single compound is different, so the above Mw / Mn range is set. In this case, the Mw / Mn distribution cannot be large, unlike the polymer.

[0203] By controlling the Mw / Mn of the compound for an organic film within such a range, an organic film having excellent filling characteristics and flatness can be formed.

[0204] Since the combination of substituents introduced into the organic film compound of the present invention can impart thermosetting properties, thermal fluidity and adhesion, an organic film excellent in heat resistance, filling / planarization properties, film forming properties and the like can be formed by using the organic film compound of the present invention.

[0205] [Method for producing compound for organic film]

[0206] In one example of the method for producing the organic film compound represented by the general formula (1) of the present invention, for example, a leaving group X having R 1 , R 2 The method of obtaining the same by using a substitution reaction with a compound (modifying agent) as a substituent, a compound having a hydroxyl group on an aromatic ring, i.e., a phenol or a compound having an amino group as a substituent on an aromatic ring, i.e., an aniline, etc., using a base catalyst. The reactions used in STEP 1 and STEP 2 can be used alone or in combination of two or more raw materials, which can be appropriately selected and combined according to the required properties. 1 , R 2 , W 1 、n 1 、n 2 As described above, X represents a halogen atom, a tosylate group, or a mesylate group.

[0207] [Phenols (STEP 1)]

[0208] [Chemistry 41]

[0209]

[0210] [Anilines (STEP 2)]

[0211] [Chemistry 42]

[0212]

[0213] When the aromatic ring has both hydroxyl and amino groups, the number of hydroxyl groups is x, the number of amino groups is y, and the number of substituents of the raw materials is adjusted to satisfy x+y=n. 1 , 2≤n 1 ≤8, 0≤x≤8, 0≤y≤8 (pattern 1). In addition, the hydroxyl group or amino group on the aromatic ring can be reacted with a variety of modifying agents in any proportion to control the introduction rate of the substituent on the hydroxyl group or amino group in any proportion. For example, when there are two substituents R 1a With R 2a , R 1b With R2b When different combinations of substituents are used, if the substituents with R 1a , R 2a The ratio of the substituent introduced is a%, and the substituent with R 1b , R 2b When the introduction ratio of the substituent is b%, the introduction rate can be controlled at any ratio so that a+b=100% (Pattern 2, Pattern 3). As in Pattern 1, even if both hydroxyl and amino groups are present, the introduction rate can still be controlled. Furthermore, even if more than three modifying agents are used, the introduction rate can still be controlled at any ratio so that the introduction rate of the substituent becomes 100%. In the following formula, W 1 , R 1 , R 2 As mentioned above, x and y are in accordance with x+y=n 1 An integer. 1a With R 2a , R 1b With R 2b For the aforementioned R 1 With R 2 Any of the following, which satisfies R 1a ≠R 1b , R 2a ≠R 2b Let n 1 The R contained as a substituent 1a , R 2a The proportion of a% is a, and the R 1b , R 2b When the ratio is b%, it meets a+b=100%, n 1a Indicates n 1 ×a÷100, n 1b Indicates n 1 ×b÷100, corresponding to n 1a +n 1b =n 1 relationship.

[0214] [Pattern 1]

[0215] [Chemistry 43]

[0216]

[0217] [Pattern 2]

[0218] [Chemistry 44]

[0219]

[0220] [Pattern 3]

[0221] [Chemistry 45]

[0222]

[0223] The base catalyst of the substitution reaction represented above, for example, inorganic base compounds such as sodium bicarbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, potassium phosphate, triethylamine, pyridine, organic amine compounds such as N-methylmorpholine, etc., can be used alone or in combination of two or more. The usage amount of this catalyst is 0.1 to 20 moles relative to the substituent group of the raw material, i.e., hydroxyl or amino, preferably in the range of 0.2 to 10 moles.

[0224] The solvent used at this time is not particularly limited as long as it is a solvent that is inactive to the above reaction, for example: ether solvents such as diethyl ether, tetrahydrofuran, dioxane, aromatic solvents such as benzene, toluene, xylene, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, water, etc., which can be used alone or in combination. These solvents can be used in the range of 0 to 2,000 parts by mass relative to 100 parts by mass of the reaction raw materials, and the reaction temperature is preferably from -50°C to the boiling point of the solvent, and more preferably from room temperature to 150°C. The reaction time can be appropriately selected from 0.1 to 100 hours.

[0225] Reaction method, there are the following methods: the method that phenols or anilines, modifiers are added to the solvent in batches, the method that phenols or anilines, modifiers are respectively or mixed, the method that the person dispersed or dissolved and feeds is added dropwise, the method that any one of phenols or anilines, modifiers is dispersed or dissolved in the solvent, the method that another person dispersed or dissolved and feeds is added dropwise, etc. In addition, when phenols or anilines, modifiers have multiple feeds respectively, the method that they are mixed in advance and reacted can also be adopted, and the method that they are reacted can also be reacted in sequence respectively. When using catalyst, the method that phenols or anilines, modifiers are added in batches, the method that catalyst is dispersed or dissolved in advance, etc. can be listed. After reaction terminates, in order to remove the unreacted raw materials, catalysts, etc. existing in the system, it is also possible to dilute in an organic solvent, utilize liquid separation cleaning, poor solvent crystallization and become powder. In addition, after dilution with an organic solvent, a solvent can be substituted into a desired organic solvent and recovered in a solution form. Furthermore, the product may be recovered in the form of a powder by crystallization or the like, and then dissolved in a desired organic solvent to be recovered in the form of a solution.

[0226] The organic solvent used for liquid separation and cleaning is not particularly limited as long as the target object can be dissolved and can be separated into two layers even when mixed with water. For example, hydrocarbons such as hexane, heptane, benzene, toluene, and xylene, esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate, ketones such as methyl ethyl ketone, methyl amyl ketone, cyclohexanone, and methyl isobutyl ketone, ethers such as diethyl ether, diisopropyl ether, methyl-tert-butyl ether, and ethyl cyclopentyl methyl ether, chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, and trichloroethylene, and mixtures thereof. The cleaning water used at this time can be what is generally called deionized water or ultrapure water. The cleaning frequency can be more than 1 time, but even if the cleaning frequency is more than 10 times, the effect of the corresponding cleaning frequency may not be obtained, so it is preferably about 1 to 5 times.

[0227] In order to remove the acidic components in the system during separation and cleaning, cleaning can also be performed with an alkaline aqueous solution. Specific examples of the alkali include alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, ammonia, and organic ammonium.

[0228] In addition, in order to remove metal impurities or alkaline components in the system during liquid separation and cleaning, cleaning can also be performed with an acidic aqueous solution. Specifically, the acid is, for example, inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, and heteropoly acids, and organic acids such as oxalic acid, fumaric acid, maleic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid.

[0229] The liquid separation and washing using the alkaline aqueous solution and the acidic aqueous solution may be performed alone or in combination. It is more preferable to perform the liquid separation and washing using the alkaline aqueous solution and the acidic aqueous solution in this order from the viewpoint of removing metal impurities.

[0230] After the above-mentioned separation and cleaning using alkaline aqueous solution and acidic aqueous solution, it is also possible to continue with cleaning with neutral water. The cleaning frequency can be more than 1 time, preferably about 1 to 5 times. Neutral water can be the deionized water, ultrapure water, etc. described above. The cleaning frequency can be more than 1 time, but sometimes the alkaline component and acidic component cannot be removed if the number of times is less. Cleaning more than 10 times may not necessarily obtain the corresponding cleaning effect, so it is preferably about 1 to 5 times.

[0231] In addition, the reaction product after the liquid separation operation can also be recovered in the form of powder by concentrating the solvent to dryness or crystallizing under reduced pressure or normal pressure. However, in order to improve the operability when preparing the organic film forming material, it can also be made into a solution state with a moderate concentration. At this time, the concentration is preferably 0.1 to 50% by mass, and more preferably 0.5 to 30% by mass. If it is such a concentration, the viscosity is not easy to increase, so the operability is not impaired, and the amount of the solvent will not become too large, so it is more economical.

[0232] The solvent at this time is not particularly limited as long as it can be a compound used for the organic film. Specific examples include ketones such as cyclohexanone and methyl-2-pentanone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono-tert-butyl ether acetate. These can be used alone or in combination of two or more.

[0233] In the preparation of the organic film-forming compound used in the organic film-forming material obtained by this method, various modifiers can be used alone or in combination according to the required performance as described above. For example, side chain structures that help improve planarization characteristics, aromatic ring structures that help etching resistance and heat resistance, etc. can be combined in any proportion. Therefore, the organic film-forming material using these organic film-forming compounds can not only take into account the filling / planarization characteristics and film forming properties, but also take into account etching in a high dimension.

[0234] As described above, according to the compound for an organic film of the present invention, an organic film-forming material which can exhibit excellent filling / planarization characteristics and film-forming properties can be provided.

[0235] In addition, the above-mentioned compound for organic film of the present invention may be used alone or in combination of two or more.

[0236] [Organic solvents]

[0237] The organic solvent that can be used in the organic film forming material of the present invention is not particularly limited as long as it can dissolve the organic film compound of the present invention and any components such as surfactants, plasticizers, acid generators, crosslinking agents, and other additives. Specifically, organic solvents having a boiling point of less than 180° C. such as the organic solvents described in paragraphs

[0091] to

[0092] of Japanese Patent Publication No. 2007-199653 can be used. Among them, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and mixtures of two or more thereof are preferably used.

[0238] Such an organic film forming material can be applied by spin coating, and contains the compound for an organic film of the present invention as described above, so it can be an organic film forming material having both heat resistance and high filling / planarization properties.

[0239] In the organic film forming material of the present invention, as for the organic solvent, a high boiling point solvent (a mixture of an organic solvent having a boiling point of less than 180°C and an organic solvent having a boiling point of more than 180°C) may be added to the organic solvent having a boiling point of less than 180°C. The high boiling point organic solvent may be any solvent capable of mixing the organic film forming compound and any surfactant, plasticizer, acid generator, crosslinking agent, other additives, etc., and is not particularly limited to hydrocarbons, alcohols, ketones, esters, ethers, chlorine-based solvents, etc. Specific examples thereof include 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, ethylene glycol, 1,2-propylene glycol, 1,3-butylene glycol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2 ,4-heptanediol, 2-ethyl-1,3-hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerol, n-nonyl acetate, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, triethylene glycol Glycol dimethyl ether, triethylene glycol monomethyl ether, triethylene glycol n-butyl ether, triethylene glycol butyl methyl ether, triethylene glycol diacetate, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin (tr iacetin), propylene glycol diacetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol methyl n-propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butanediol diacetate, 1,6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, dibutyl adipate, etc., which can be used alone or in combination.

[0240] The boiling point of the high boiling point solvent can be appropriately selected in accordance with the temperature at which the organic film forming material is subjected to heat treatment. The boiling point of the added high boiling point solvent is preferably 180°C to 300°C, and more preferably 200°C to 300°C. If the boiling point is such, there is no risk of excessively rapid volatilization during baking (heat treatment) due to a too low boiling point, and sufficient thermal fluidity can be obtained. Furthermore, if the boiling point is such, there is no risk of non-volatile residues remaining in the film after baking due to a too high boiling point, and there is no risk of adverse effects on film properties such as etching resistance.

[0241] When the high boiling point solvent is used, the blending amount of the high boiling point solvent is preferably 1 to 30 parts by mass based on 100 parts by mass of the organic solvent having a boiling point of less than 180° C. If the blending amount is such, there is no risk that the blending amount is too small and sufficient heat flow cannot be imparted during baking, or that the blending amount is too large and remains in the film, thereby causing deterioration of film properties such as etching resistance.

[0242] Such an organic film forming material can be obtained by adding a high boiling point solvent to the above-mentioned organic film forming compound to impart thermal fluidity, thereby achieving both high filling and planarizing properties.

[0243] In the present invention, the organic film-forming material preferably contains one or more of a surfactant and a plasticizer.

[0244] [Surfactant]

[0245] The organic film-forming material of the present invention may contain a surfactant to improve the coating properties of spin coating. As the surfactant, for example, the surfactants described in paragraphs

[0142] to

[0147] of JP-A-2009-269953 may be used.

[0246] The above-mentioned surfactant may be used alone or in combination of two or more thereof. The amount of the surfactant added is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the compound for organic membrane.

[0247] [Plasticizer]

[0248] In addition, in the organic film forming material of the present invention, a plasticizer may be added to further improve the planarization / burying characteristics. There is no particular limitation on the plasticizer, and plasticizers of various known systems can be widely used. For example, low molecular weight compounds such as phthalates, adipic acid esters, phosphates, trimellitic acid esters, and citrates, polyethers, polyesters, and polymers such as polyacetal polymers described in Japanese Patent Publication No. 2013-253227. The amount of the plasticizer added is preferably 1 to 100 parts by mass, and more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the aforementioned organic film compound.

[0249] In addition, in the organic film forming material of the present invention, as an additive that imparts the same filling / planarizing properties as the plasticizer, it is preferable to use, for example, a liquid additive having a polyethylene glycol or polypropylene glycol structure, or a pyrolyzable polymer having a weight loss rate of 40% by mass or more between 30°C and 250°C and a weight average molecular weight of 300 to 200,000. The pyrolyzable polymer preferably contains a repeating unit having an acetal structure represented by the following general formula (DP1) or (DP1a). The amount of these pyrolyzable polymers added is preferably 1 to 100 parts by mass, more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the aforementioned organic film compound.

[0250] [Chemistry 46]

[0251]

[0252] In the formula, R a is a hydrogen atom or an optionally substituted saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms. L is a saturated or unsaturated divalent organic group having 2 to 30 carbon atoms.

[0253] [Chemistry 47]

[0254]

[0255] In the formula, R b is an alkyl group having 1 to 4 carbon atoms. Z is a saturated or unsaturated divalent hydrocarbon group having 4 to 10 carbon atoms, and may have an ether bond. t represents the average number of repeating units, and is 3 to 500.

[0256] In addition, the following fluidity promoters may be used as additives for improving the same filling / planarization characteristics as described above. The fluidity promoter may be selected from one or more compounds of the following general formulas (i) to (iii). The amount of these fluidity promoters added is preferably 1 to 100 parts by mass, more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the aforementioned organic film compound.

[0257] [Chemistry 48]

[0258]

[0259] In the formula, R c Each independently represents a hydrogen atom, a hydroxyl group, or an optionally substituted organic group having 1 to 10 carbon atoms. a W is a phenylene group or a divalent group represented by the following general formula (i-1). b , W c is a single bond or a divalent group represented by the following formula (i-2). a is an integer from 1 to 10, n a An integer from 0 to 5.

[0260] [Chemistry 49]

[0261]

[0262] In the formula, * represents the bonding position, R d , R e , R f , R g W is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms. d , W e Each independently represents a single bond or a carbonyl group. b 、m c is an integer from 0 to 10, m b +m c ≥1.

[0263] [Chemistry 50]

[0264]

[0265] In the formula, * represents the bonding position.

[0266] [Chemistry 51]

[0267]

[0268] In the formula, R h Each independently represents a hydrogen atom or an optionally substituted organic group having 1 to 10 carbon atoms. f W is a divalent group represented by the following general formula (ii-1). g is a single bond or a divalent group represented by the following formula (ii-2). d is an integer from 2 to 10, n b An integer from 0 to 5.

[0269] [Chemistry 52]

[0270]

[0271] In the formula, * represents the bonding position, R i , R j , R k , R l is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms. e 、m f is an integer from 0 to 10, m e +m f ≥1.

[0272] [Chemistry 53]

[0273]

[0274] In the formula, * represents the bonding position.

[0275] [Chemistry 54]

[0276]

[0277] In the formula, R m , R n R is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms which may be substituted, and may be bonded to each other to form a ring structure. o , R p is an organic group having 1 to 10 carbon atoms, R o W is a group containing an aromatic ring or a divalent group represented by the following general formula (iii-1). g , W h It is a single bond or a divalent group represented by the following formula (iii-2), and at least one of them is a divalent group represented by the following formula (iii-2).

[0278] [Chemistry 55]

[0279]

[0280] In the formula, * represents the bonding position, W i It is an organic group having 1 to 4 carbon atoms.

[0281] [Chemistry 56]

[0282]

[0283] In the formula, * represents the bonding position.

[0284] [Acid generator]

[0285] In order to further promote the curing reaction, an acid generator may be added to the organic film forming material of the present invention. Acid generators may generate acid by thermal decomposition or by light irradiation, and both may be added. Specifically, materials described in paragraphs

[0061] to

[0085] of Japanese Patent Publication No. 2007-199653 may be added, but are not limited thereto.

[0286] The acid generator may be used alone or in combination of two or more. The amount of the acid generator added is preferably 0.05 to 50 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the compound for an organic film.

[0287] [Crosslinking agent]

[0288] In addition, in the organic film forming material of the present invention, a crosslinking agent may be added in order to improve the hardening property and further suppress the cross-mixing with the upper film of the resist. The crosslinking agent is not particularly limited, and various well-known crosslinking agents can be widely used. For example, melamine crosslinking agents, glycoluril crosslinking agents, benzoguanamine crosslinking agents, urea crosslinking agents, β-hydroxyalkylamide crosslinking agents, isocyanurate crosslinking agents, aziridine crosslinking agents, oxazoline crosslinking agents, epoxy crosslinking agents, and polynuclear phenol crosslinking agents.

[0289] Specific examples of the melamine-based crosslinking agent include hexamethoxymethylated melamine, hexabutoxymethylated melamine, alkoxy and / or hydroxyl-substituted melamines thereof, and partially self-condensed products thereof.

[0290] Specific examples of the glycoluril-based crosslinking agent include tetramethoxymethyl glycoluril, tetrabutoxymethyl glycoluril, alkoxy and / or hydroxyl-substituted products thereof, and partial self-condensation products thereof.

[0291] Specific examples of the benzoguanamine-based crosslinking agent include tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, alkoxy and / or hydroxyl-substituted products thereof, and partial self-condensation products thereof.

[0292] Specific examples of the urea crosslinking agent include dimethoxymethylated dimethoxyethylene urea, alkoxy and / or hydroxyl substituted products thereof, and partial self-condensation products thereof.

[0293] Specific examples of the β-hydroxyalkylamide crosslinking agent include N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide.

[0294] Specific examples of the isocyanurate crosslinking agent include triglycidyl isocyanurate and triallyl isocyanurate.

[0295] Specific examples of the aziridine crosslinking agent include 4,4′-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate.

[0296] Oxazoline crosslinking agents include, for example, 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis-4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tert-butyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymers.

[0297] Specific examples of the epoxy crosslinking agent include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.

[0298] The polynuclear phenol-based crosslinking agent is specifically, for example, a compound represented by the following general formula (1A).

[0299] [Chemistry 57]

[0300]

[0301] In the formula, Q is a single bond or an S-valent hydrocarbon group having 1 to 20 carbon atoms. 10 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. s is an integer of 1 to 5.

[0302] Q is a single bond or an s-valent hydrocarbon group having 1 to 20 carbon atoms. s is an integer of 1 to 5, preferably 2 or 3. Specifically, Q is a group obtained by removing q hydrogen atoms from methane, ethane, propane, butane, isobutane, pentane, cyclopentane, hexane, cyclohexane, methylpentane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, benzene, toluene, xylene, ethylbenzene, ethylisopropylbenzene, diisopropylbenzene, methylnaphthalene, ethylnaphthalene, or eicosane. R 10 It is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specifically, the alkyl group having 1 to 20 carbon atoms includes methyl, ethyl, propyl, isopropyl, butyl, isobutyl, pentyl, isopentyl, hexyl, octyl, ethylhexyl, decyl and eicosyl, and a hydrogen atom or a methyl group is preferred.

[0303] Examples of compounds represented by the general formula (1A) include the following compounds. Among them, from the perspective of improving the hardening property and film thickness uniformity of the organic film, hexamethoxymethylated products of trisphenolmethane, trisphenolethane, 1,1,1-tris(4-hydroxyphenyl)ethane, and tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene are preferred. 10 Same as above.

[0304] [Chemistry 58]

[0305]

[0306] [Chemistry 59]

[0307]

[0308] The crosslinking agent may be used alone or in combination of two or more. The amount of the crosslinking agent added is preferably 1 to 100 parts by mass, more preferably 5 to 50 parts by mass, based on 100 parts by mass of the compound for an organic film.

[0309] [Other ingredients]

[0310] The organic film forming material of the present invention may be mixed with other compounds or polymers. The compound or polymer is mixed with the organic film forming material of the present invention and plays a role in improving the film forming property of spin coating and the filling property of substrates with height differences.

[0311] Such materials, for example, phenol, o-cresol, m-cresol, p-cresol, 2,3-dimethylphenol, 2,5-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2,4-dimethylphenol, 2,6-dimethylphenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, 2-tert-butylphenol, 3-tert-butylphenol, 4-tert-butylphenol, 2-phenylphenol, 3-phenylphenol, 4-phenylphenol, 3,5-diphenylphenol, 2-naphthylphenol, 3-naphthylphenol, 4-naphthylphenol, 4-tritylphenol, resorcinol, 2-methylresorcinol, 4-methylresorcinol, 5-methylresorcinol, catechol, 4-tert-butylcatechol, 2 -Methoxyphenol, 3-methoxyphenol, 2-propylphenol, 3-propylphenol, 4-propylphenol, 2-isopropylphenol, 3-isopropylphenol, 4-isopropylphenol, 2-methoxy-5-methylphenol, 2-tert-butyl-5-methylphenol, gallol, thymol, isothymol, 4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-dimethyl-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-diallyl-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-difluoro-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-diphenyl-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-dimethoxy 4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 3,3,3',3'-tetramethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 3,3,3',3',4,4'-hexamethyl-2 ,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 2,3,2',3'-tetrahydro-(1,1')-spirobiindene-5,5'-diol, 5,5'-dimethyl-3,3,3',3'-tetramethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 1- Naphthol, 2-naphthol, 2-methyl-1-naphthol, 4-methoxy-1-naphthol, 7-methoxy-2-naphthol and dihydroxynaphthalene such as 1,5-dihydroxynaphthalene, 1,7-dihydroxynaphthalene and 2,6-dihydroxynaphthalene, methyl 3-hydroxynaphthalene-2-carboxylate, indene, hydroxyindene, benzofuran, hydroxyanthracene, vinylnaphthalene, biphenyl, bisphenol, triphenol, dicyclopentadiene, tetrahydroindene, 4-vinylcyclohexene, norbornene, 5-vinylnorbornene-2-ene, α-pinene, β-pinene, limonene and other novolac resins, polyhydroxystyrene, polystyrene, polyvinylnaphthalene, polyvinylanthracene, polyvinylcarbazole, polyindene, polyvinylnaphthalene, polynorbornene, polycyclodecene, polytetracyclododecene, polytricyclo[2.2.1.0(2,6)]heptane (poly-nortricyclene), poly(meth)acrylate and copolymers thereof. In addition, naphthol dicyclopentadiene copolymers described in Japanese Patent Application Laid-Open No. 2004-205685, fluorene bisphenol novolac resins described in Japanese Patent Application Laid-Open No. 2005-128509, ethylene naphthalene copolymers described in Japanese Patent Application Laid-Open No. 2005-250434, fullerenes having phenol groups described in Japanese Patent Application Laid-Open No. 2006-227391, bisphenol compounds and novolac resins thereof described in Japanese Patent Application Laid-Open No. 2006-293298, adamantane phenol compounds and novolac resins thereof described in Japanese Patent Application Laid-Open No. 2006-285095, bisnaphthol compounds and novolac resins thereof described in Japanese Patent Application Laid-Open No. 2010-122656, fullerene resin compounds described in Japanese Patent Application Laid-Open No. 2008-158002, etc. may also be blended.

[0312] The blending amount of the compound for doping or the polymer for doping is preferably 0 to 1,000 parts by mass, more preferably 0 to 500 parts by mass, based on 100 parts by mass of the compound for organic membrane.

[0313] The organic film forming material can be used as an organic film material or a planarizing material for manufacturing a semiconductor device.

[0314] In addition, the organic film forming material of the present invention is extremely useful as an organic film material for multilayer resist processing, such as a two-layer resist processing, a three-layer resist processing using a silicon-containing resist intermediate film, and a four-layer resist processing using a silicon-containing inorganic hard mask intermediate film and an organic antireflective film.

[0315] <Organic film formation method>

[0316] Furthermore, by using the above-mentioned organic film forming material, an organic film serving as a multilayer resist film used in photolithography or an organic film serving as a planarizing film for semiconductor manufacturing can be formed.

[0317] In the organic film forming method using the organic film forming material of the present invention, the above-mentioned organic film forming material can be coated on the processed substrate (processed body) by spin coating or the like. By using the spin coating method or the like, good filling characteristics can be obtained. After spin coating, the organic solvent is evaporated, and baking (heat treatment) is performed to prevent mixing with the resist upper film and the resist intermediate film and to promote the cross-linking reaction. The baking is preferably performed in the range of 100°C to 600°C for 10 to 600 seconds, and more preferably in the range of 200°C to 500°C for 10 to 300 seconds. Considering the damage to the device and the influence on the deformation of the wafer, the upper limit of the heating temperature in the wafer processing of the lithography is preferably set to be below 600°C, and more preferably below 500°C.

[0318] In addition, an organic film forming method using the organic film forming material of the present invention can coat the organic film forming material of the present invention on a processed substrate by the same spin coating method as mentioned above, and the above-mentioned organic film forming material is fired in a gas environment with an oxygen concentration of not less than 0.1% and not more than 21% to harden it, so as to form an organic film.

[0319] By firing the organic film forming material of the present invention in such an oxygen atmosphere, a sufficiently hardened organic film can be obtained. The gas atmosphere during the baking process may be air, but in order to reduce oxygen, N 2 Inert gases such as Ar, He, etc. are ideal for preventing oxidation of organic films. In order to prevent oxidation, the oxygen concentration needs to be controlled, preferably below 1,000 ppm, more preferably below 100 ppm. If the organic film is prevented from oxidizing during baking, there will be no increase in absorption or decrease in etching resistance, so it is ideal.

[0320] The organic film forming method using the organic film forming material of the present invention can obtain a flat cured film regardless of the unevenness of the processed substrate due to its excellent filling / flattening properties. Therefore, it is very useful when forming a flat organic film on a processed substrate with a structure having a height of more than 30nm or a height difference.

[0321] The thickness of the organic film or the organic film such as the planarization film for manufacturing a semiconductor device can be appropriately selected, and is preferably 30 to 20,000 nm, and more preferably 50 to 15,000 nm.

[0322] <Pattern Formation Method>

[0323] In the present invention, as a pattern forming method by three-layer resist processing using such an organic film forming material, a pattern forming method is provided, which is a method for forming a pattern on a processed substrate, at least

[0324] forming an organic film on a workpiece using the organic film forming material described above,

[0325] On the organic film, a silicon-containing resist intermediate film is formed using a silicon-containing resist intermediate film material.

[0326] A photoresist composition is used to form a resist upper film on the silicon-containing resist intermediate film.

[0327] forming a circuit pattern on the resist upper film,

[0328] The pattern is transferred to the silicon-containing resist intermediate film by etching using the patterned resist upper film as a mask.

[0329] The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film having the transferred pattern as a mask.

[0330] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0331] The silicon-containing resist intermediate film in the above-mentioned three-layer resist treatment shows resistance to etching using oxygen or hydrogen. Therefore, in the above-mentioned three-layer resist treatment, dry etching of the organic film using the silicon-containing resist intermediate film as a mask is preferably carried out using an etching gas mainly composed of oxygen or hydrogen.

[0332] The silicon-containing resist intermediate film for the above-mentioned three-layer resist treatment is also preferably a polysiloxane-based intermediate film. By giving the silicon-containing resist intermediate film an anti-reflection effect, reflection can be suppressed. In particular, for 193nm exposure, if the organic film uses a material containing many aromatic groups and having a high etching selectivity with the substrate, the k value is high and the substrate reflection is high. However, by having an absorption with an appropriate k value for the silicon-containing resist intermediate film, reflection can be suppressed and the substrate reflection can be made less than 0.5%. For the silicon-containing resist intermediate film with an anti-reflection effect, it is more ideal to use anthracene for 248nm and 157nm exposure, and to use a polysiloxane with a pendant phenyl group or a light-absorbing group with a silicon-silicon bond for 193nm exposure and cross-linked with acid or heat.

[0333] In addition, a pattern forming method is provided, which is also suitable for a four-layer resist process using an organic anti-reflection film, in which case, at least a method for forming a pattern on a workpiece is provided.

[0334] forming an organic film on a workpiece using the organic film forming material described above,

[0335] On the organic film, a silicon-containing resist intermediate film is formed using a silicon-containing resist intermediate film material.

[0336] forming an organic anti-reflective film (BARC) on the aforementioned silicon-containing resist intermediate film,

[0337] On the aforementioned BARC, a resist upper layer film is formed using a photoresist composition to form a 4-layer film structure.

[0338] forming a circuit pattern on the resist upper film,

[0339] The aforementioned patterned resist upper layer film is used as a mask, and the aforementioned BARC is transferred to the aforementioned silicon-containing resist intermediate film by etching.

[0340] The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film having the transferred pattern as a mask.

[0341] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0342] Furthermore, an inorganic hard mask intermediate film may be formed instead of the silicon-containing resist intermediate film. In this case, a pattern forming method is provided, which is at least a method for forming a pattern on a workpiece.

[0343] forming an organic film on a workpiece using the organic film forming material described above,

[0344] On the aforementioned organic film, an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film is formed;

[0345] On the inorganic hard mask intermediate film, a resist upper layer film is formed using a photoresist composition.

[0346] forming a circuit pattern on the resist upper film,

[0347] The pattern is transferred to the inorganic hard mask intermediate film by etching using the patterned resist upper film as a mask.

[0348] The inorganic hard mask intermediate film with the transferred pattern is used as a mask to transfer the pattern to the organic film by etching.

[0349] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0350] As described above, when an inorganic hard mask intermediate film is formed on an organic film, a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film (SiON film) can be formed by a CVD method, an ALD method, or the like. For example, a method for forming a silicon nitride film is described in Japanese Patent Application Publication No. 2002-334869 and International Publication No. 2004 / 066377. The film thickness of the inorganic hard mask intermediate film is preferably 5 to 200 nm, and more preferably 10 to 100 nm. In addition, as for the inorganic hard mask intermediate film, it is most preferable to use a SiON film that has a high effect as an anti-reflective film. Since the substrate temperature when forming the SiON film is 300 to 500°C, the organic film needs to withstand a temperature of 300 to 500°C. The organic film forming material used in the present invention has high heat resistance and can withstand a high temperature of 300 to 500°C, so it can be a combination of an inorganic hard mask intermediate film formed by a CVD method or an ALD method and an organic film formed by a spin coating method.

[0351] Furthermore, it is also suitable for a four-layer resist process using an organic antireflection film. In this case, a pattern forming method is provided, which is at least a method for forming a pattern on a workpiece.

[0352] forming an organic film on a workpiece using the organic film forming material described above,

[0353] On the aforementioned organic film, an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film is formed;

[0354] On the inorganic hard mask intermediate film, an organic anti-reflection film (BARC) is formed.

[0355] On the aforementioned BARC, a resist upper layer film is formed using a photoresist composition to form a 4-layer film structure.

[0356] forming a circuit pattern on the resist upper film,

[0357] The patterned resist upper film is used as a mask, and the BARC is etched to transfer the pattern to the inorganic hard mask intermediate film.

[0358] The inorganic hard mask intermediate film with the transferred pattern is used as a mask to transfer the pattern to the organic film by etching.

[0359] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0360] As described above, a photoresist film as a resist upper film may be formed on the inorganic hard mask intermediate film, and an organic antireflection film (BARC) may be formed on the inorganic hard mask intermediate film by spin coating and a photoresist film may be formed thereon. In particular, when a SiON film is used as the inorganic hard mask intermediate film, the two-layer antireflection film of the SiON film and the BARC can suppress reflection even in immersion exposure with a high NA exceeding 1.0. Another benefit of forming the BARC is that it has the effect of reducing the tailing of the photoresist pattern directly on the SiON film.

[0361] The resist upper film of the above three-layer resist treatment can be either positive or negative, and can use the same photoresist composition as commonly used. After spin coating, the photoresist composition is pre-baked, preferably at 60 to 180° C. for 10 to 300 seconds. Thereafter, exposure is performed according to the usual method, and then post-exposure baking (PEB) and development are performed to obtain a resist pattern. In addition, the thickness of the resist upper film is not particularly limited, and 30 to 500 nm is ideal, and 50 to 400 nm is particularly preferred.

[0362] The exposure light may be, for example, high-energy radiation having a wavelength of 300 nm or less, specifically, excimer lasers of 248 nm, 193 nm, and 157 nm, soft X-rays of 3 to 20 nm, electron beams, and X-rays.

[0363] The patterning method of the resist upper layer film is preferably a patterning method using optical lithography with a wavelength of 10 nm to 300 nm, direct writing using an electron beam, nanoimprinting, or a combination thereof.

[0364] Furthermore, the developing method in the above-mentioned pattern forming method is preferably alkali developing or organic solvent developing.

[0365] Then, etching is performed using the obtained resist upper film pattern as a mask. In the three-layer resist process, etching of the silicon-containing resist intermediate film and the inorganic hard mask intermediate film is performed using a fluorocarbon-based gas and the resist upper film pattern as a mask. In this way, a silicon-containing resist intermediate film pattern and an inorganic hard mask intermediate film pattern are formed.

[0366] Next, the organic film is etched using the obtained silicon-containing resist interlayer film pattern and inorganic hard mask interlayer film pattern as masks.

[0367] The etching of the substrate to be processed (the object to be processed) can also be carried out by conventional methods. For example, if the substrate to be processed is SiO 2 For low dielectric constant insulating films of SiN and silicon dioxide, etching is mainly performed with fluorine-based gases, and etching is mainly performed with chlorine-based and bromine-based gases for p-Si, Al, and W. When etching is performed with fluorine-based gases during substrate processing, the silicon-containing resist intermediate film pattern will be stripped off during the three-layer resist processing while the substrate is being processed. When etching the substrate with chlorine-based and bromine-based gases, the stripping of the silicon-containing resist intermediate film pattern must be performed separately after substrate processing by dry etching stripping using fluorine-based gases.

[0368] The organic film obtained by using the organic film forming material of the present invention has a characteristic of being excellent in etching resistance when etching these substrates to be processed.

[0369] The workpiece is preferably a semiconductor device substrate, or a semiconductor device substrate having a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon. More specifically, Si, α-Si, p-Si, SiO 2 , SiN, SiON, W, TiN, Al and other substrates, and those having the above-mentioned metal films formed on the above-mentioned substrates as processed layers, etc.

[0370] The processed layer can use Si, SiO 2, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si and other Low-k films and barrier films thereof can be formed with a thickness of 50 to 10,000 nm, especially 100 to 5,000 nm. In addition, when forming the processed layer, the substrate and the processed layer can be made of different materials.

[0371] Furthermore, the aforementioned metal is preferably silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, manganese, molybdenum, ruthenium or an alloy thereof.

[0372] Furthermore, it is preferable that the substrate to be processed has a structure with a height of 30 nm or more or a height difference.

[0373] An example of a 3-layer resist process using Figure 1 The details are as follows. When the 3-layer resist is processed, Figure 1 As shown in (A), an organic film 3 is formed on a processing layer 2 stacked on a substrate 1 using the organic film forming material of the present invention, and then a silicon-containing resist intermediate film 4 is formed and a resist upper film 5 is formed thereon.

[0374] Secondly, if Figure 1 As shown in (B), the important part 6 of the resist upper film 5 is exposed, PEB and development are performed, as shown in FIG. Figure 1 As shown in (C), the resist upper film pattern 5a is formed. Using the obtained resist upper film pattern 5a as a mask, the silicon-containing resist intermediate film 4 is etched using CF system gas, as shown in FIG. Figure 1 As shown in (D), a silicon-containing resist intermediate film pattern 4a is formed. After the resist upper film pattern 5a is removed, the obtained silicon-containing resist intermediate film pattern 4a is used as a mask to perform oxygen plasma etching on the organic film 3, as shown in FIG. Figure 1 As shown in (E), an organic film pattern 3a is formed. After the silicon-containing resist intermediate film pattern 4a is removed, the processed layer 2 is etched using the organic film pattern 3a as a mask, as shown in FIG. Figure 1 As shown in (F), pattern 2a is formed.

[0375] When an inorganic hard mask interlayer is used, the silicon-containing resist interlayer 4 is an inorganic hard mask interlayer, and when BARC is applied, BARC is provided between the silicon-containing resist interlayer 4 and the resist upper film 5. BARC etching may be performed continuously before etching the silicon-containing resist interlayer 4, or etching of the silicon-containing resist interlayer 4 may be performed after etching of BARC alone, and etching equipment may be changed.

[0376] As described above, according to the pattern forming method of the present invention, a fine pattern can be formed on a substrate to be processed with high precision in a multilayer resist process.

[0377] Example

[0378] The following synthesis examples, embodiments, and comparative examples are provided to more specifically describe the present invention, but the present invention is not limited thereto. In addition, the molecular weight and the dispersity are determined by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent to obtain a weight average molecular weight (Mw) and a number average molecular weight (Mn) in terms of polystyrene, and to obtain a dispersity (Mw / Mn).

[0379] [Synthesis of Compounds (A1) to (A25) for Organic Films in Synthesis Example and Compounds (R1) to (R3) for Comparative Example]

[0380] The organic film compounds (A1) to (A25) were synthesized using the following compounds (B1) to (B12) having amino groups or hydroxy groups and the modifying agents (C1) to (C8). The comparative compound (R3) was synthesized using the comparative compound raw material (D1).

[0381] Compounds with amino and hydroxyl groups:

[0382] [Chemistry 60]

[0383]

[0384] Modifying agent:

[0385] [Chemistry 61]

[0386]

[0387] Comparative Example Compound Raw Materials:

[0388] [Chemistry 62]

[0389]

[0390] (Synthesis example 1)

[0391] Synthesis of Compound (A1) for Organic Membrane

[0392] [Chemistry 63]

[0393]

[0394] Under nitrogen atmosphere, add 10.0 g of compound (B1), 38.5 g of potassium carbonate, and 140 g of DMF (dimethylformamide) to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop a solution prepared by mixing 45.8 g of the modifying agent (C1) and 180 g of DMF and homogenizing them in advance, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 500 g of MIBK (methyl isobutyl ketone) and 500 g of pure water to prepare a uniform solution, and then remove the aqueous layer. Wash the organic layer twice with 200 g of 3.0% nitric acid aqueous solution and 5 times with 200 g of pure water, and dry the organic layer under reduced pressure. Add 110 g of THF to the residue to prepare a uniform solution, and then drop it into 700 g of hexane to crystallize. The crystals that have crystallized are separated by filtration, washed twice with 200 g of hexane, and recovered. The recovered crystals were vacuum dried at 70°C to obtain a compound for an organic membrane (A1).

[0395] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0396] (A1): Mw=840, Mw / Mn=1.02

[0397] (Synthesis example 2)

[0398] Synthesis of Compound (A2) for Organic Membrane

[0399] [Chemistry 64]

[0400]

[0401] Under nitrogen atmosphere, add 10.0 g of compound (B1), 38.5 g of potassium carbonate and 140 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 67.5 g of the modifying agent (C5) and 270 g of DMF, which are pre-mixed and homogenized to obtain a solution, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 500 g of MIBK and 500 g of pure water to prepare a uniform solution, and then remove the aqueous layer. Wash the organic layer twice with 200 g of 3.0% nitric acid aqueous solution, and wash 5 times with 200 g of pure water, and dry the organic layer under reduced pressure. Add 170 g of THF to the residue to prepare a uniform solution, and then drop 1000 g of methanol to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 300 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain the compound (A2) for organic membrane.

[0402] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0403] (A2): Mw=1,200, Mw / Mn=1.01

[0404] (Synthesis example 3)

[0405] Synthesis of Compound (A3) for Organic Membrane

[0406] [Chemistry 65]

[0407]

[0408] Under nitrogen atmosphere, add 10.0 g of compound (B2), 14.2 g of potassium carbonate and 75 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 22.3 g of the modifying agent (C2) and 70 g of DMF, which are pre-mixed and homogenized, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 300 g of MIBK and 300 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 100 g of 3.0% nitric acid aqueous solution and 5 times with 100 g of pure water, and dry the organic layer under reduced pressure. Add 70 g of THF to the residue, and after it becomes a uniform solution, add dropwise to 400 g of hexane to crystallize. The crystallized crystals are separated by filtration, washed twice with 100 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A3) for organic membrane.

[0409] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0410] (A3): Mw=710, Mw / Mn=1.01

[0411] (Synthesis Example 4)

[0412] Synthesis of Compound (A4) for Organic Membrane

[0413] [Chemistry 66]

[0414]

[0415] Under nitrogen environment, add 10.0 g of compound (B2), 14.2 g of potassium carbonate, and 75 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 24.8 g of the modifying agent (C5) and 75 g of DMF, which are pre-mixed and homogenized to obtain a solution, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 300 g of MIBK and 300 g of pure water. After a uniform solution is obtained, remove the aqueous layer. Wash the organic layer twice with 100 g of 3.0% nitric acid aqueous solution and 5 times with 100 g of pure water, and dry the organic layer under reduced pressure. Add 80 g of THF to the residue, and after it becomes a uniform solution, add dropwise to 500 g of methanol to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 100 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A4) for organic membrane.

[0416] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0417] (A4): Mw=780, Mw / Mn=1.02

[0418] (Synthesis Example 5)

[0419] Synthesis of Compound (A5) for Organic Membrane

[0420] [Chemistry 67]

[0421]

[0422] Under nitrogen atmosphere, add 10.0 g of compound (B3), 20.8 g of potassium carbonate and 120 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 31.9 g of the modifying agent (C3) and 100 g of DMF, which are pre-mixed and homogenized to obtain a solution, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 300 g of MIBK and 300 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 100 g of 3.0% nitric acid aqueous solution and 5 times with 100 g of pure water, and dry the organic layer under reduced pressure. Add 90 g of THF to the residue, and after it becomes a uniform solution, add 550 g of hexane dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 100 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A5) for organic membrane.

[0423] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0424] (A5): Mw=1,260, Mw / Mn=1.02

[0425] (Synthesis Example 6)

[0426] Synthesis of Compound (A6) for Organic Membrane

[0427] [Chemistry 68]

[0428]

[0429] Under nitrogen atmosphere, add 10.0 g of compound (B3), 20.8 g of potassium carbonate and 120 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 42.0 g of the modifying agent (C6) and 130 g of DMF, which are pre-mixed and homogenized to obtain a solution, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 400 g of MIBK and 400 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 120 g of THF to the residue, and after it becomes a uniform solution, add 600 g of methanol dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 150 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A6) for organic membrane.

[0430] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0431] (A6): Mw=1,630, Mw / Mn=1.01

[0432] (Synthesis Example 7)

[0433] Synthesis of Compound (A7) for Organic Membrane

[0434] [Chemistry 69]

[0435]

[0436] Under nitrogen atmosphere, add 10.0 g of compound (B4), 16.2 g of potassium carbonate and 80 g of DMF, and prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 24.9 g of the modifying agent (C3) and 75 g of DMF, which are pre-mixed and homogenized to obtain a solution, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 200 g of MIBK and 200 g of pure water, and after a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 100 g of 3.0% nitric acid aqueous solution and 5 times with 100 g of pure water, and dry the organic layer under reduced pressure. Add 75 g of THF to the residue, and after it becomes a uniform solution, add dropwise to 400 g of hexane to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 100 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A7) for organic membrane.

[0437] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0438] (A7): Mw=890, Mw / Mn=1.01

[0439] (Synthesis Example 8)

[0440] Synthesis of Compound (A8) for Organic Membrane

[0441] [Chemistry 70]

[0442]

[0443] Under nitrogen atmosphere, add 10.0 g of compound (B4), 16.2 g of potassium carbonate and 80 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop the solution obtained by pre-mixing and homogenizing the modifying agent (C4) 29.0 g and DMF 90 g, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 200 g of MIBK and 200 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 100 g of 3.0% nitric acid aqueous solution and 5 times with 100 g of pure water, and dry the organic layer under reduced pressure. Add 90 g of THF to the residue to form a uniform solution, then drop it in 450 g of hexane to crystallize. The crystallized crystals are separated by filtration, washed twice with 100 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A8) for organic membrane.

[0444] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0445] (A8): Mw=980, Mw / Mn=1.02

[0446] (Synthesis Example 9)

[0447] Synthesis of Compound (A9) for Organic Membrane

[0448] [Chemistry 71]

[0449]

[0450] Under nitrogen atmosphere, add 10.0 g of compound (B5), 11.5 g of potassium carbonate and 60 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop the solution obtained by pre-mixing and homogenizing the modifying agent (C2) 18.0 g and DMF 75 g, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 200 g of MIBK and 200 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 100 g of 3.0% nitric acid aqueous solution and 5 times with 100 g of pure water, and dry the organic layer under reduced pressure. Add 65 g of THF to the residue, and after it becomes a uniform solution, add dropwise to 400 g of hexane to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 100 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A9) for organic membrane.

[0451] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0452] (A9): Mw=1,080, Mw / Mn=1.02

[0453] (Synthesis Example 10)

[0454] Synthesis of Compound (A10) for Organic Membrane

[0455] [Chemistry 72]

[0456]

[0457] Under nitrogen atmosphere, add 10.0 g of compound (B5), 11.5 g of potassium carbonate and 60 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 29.2 g of the modifying agent (C7) and 90 g of DMF, which are pre-mixed and homogenized, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 300 g of MIBK and 200 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 100 g of 3.0% nitric acid aqueous solution and 5 times with 100 g of pure water, and dry the organic layer under reduced pressure. Add 90 g of THF to the residue, and after it becomes a uniform solution, add 400 g of methanol dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 100 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain a compound (A10) for organic membranes.

[0458] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0459] (A10): Mw=1,540, Mw / Mn=1.03

[0460] (Synthesis Example 11)

[0461] Synthesis of Compound (A11) for Organic Membrane

[0462] [Chemistry 73]

[0463]

[0464] Under nitrogen atmosphere, add 10.0 g of compound (B6), 21.8 g of potassium carbonate and 100 g of DMF, and prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 33.4 g of the modifying agent (C3) and 130 g of DMF, which are pre-mixed and homogenized, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 400 g of MIBK and 300 g of pure water, and after a uniform solution is formed, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution, and wash 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 100 g of THF to the residue, and after it becomes a uniform solution, add dropwise to 400 g of hexane to crystallize. The crystallized crystals are separated by filtration, washed twice with 100 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain a compound (A11) for organic membranes.

[0465] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0466] (A11): Mw=1,220, Mw / Mn=1.03

[0467] (Synthesis Example 12)

[0468] Synthesis of Compound (A12) for Organic Membrane

[0469] [Chemistry 74]

[0470]

[0471] Under nitrogen atmosphere, add 10.0 g of compound (B6), 21.8 g of potassium carbonate and 100 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 54.0 g of the modifying agent (C8) and 160 g of DMF, which are pre-mixed and homogenized, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 400 g of MIBK and 300 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 140 g of THF to the residue, and after a uniform solution is obtained, add 500 g of methanol dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 200 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain a compound (A12) for organic membranes.

[0472] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0473] (A12): Mw=1,920, Mw / Mn=1.03

[0474] (Synthesis Example 13)

[0475] Synthesis of Compound (A13) for Organic Membrane

[0476] [Chemistry 75]

[0477]

[0478] Under nitrogen atmosphere, add 10.0 g of compound (B7), 27.8 g of potassium carbonate and 120 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop the solution obtained by pre-mixing and homogenizing 43.6 g of the modifying agent (C2) and 130 g of DMF, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 400 g of MIBK and 400 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 110 g of THF to the residue, and after it becomes a uniform solution, add 500 g of hexane dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 150 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain a compound (A13) for organic membranes.

[0479] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0480] (A13): Mw=1,550, Mw / Mn=1.01

[0481] (Synthesis Example 14)

[0482] Synthesis of Compound (A14) for Organic Membrane

[0483] [Chemistry 76]

[0484]

[0485] Under nitrogen atmosphere, add 10.0 g of compound (B7), 27.8 g of potassium carbonate, and 120 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 56.1 g of the modifying agent (C6) and 170 g of DMF, which are pre-mixed and homogenized, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 500 g of MIBK and 400 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 140 g of THF to the residue, and after a uniform solution is obtained, add 600 g of methanol dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 150 g of methanol, and recovered. The recovered crystals are vacuum dried at 70°C to obtain the compound (A14) for organic membrane.

[0486] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0487] (A14): Mw=1,900, Mw / Mn=1.02

[0488] (Synthesis Example 15)

[0489] Synthesis of Compound (A15) for Organic Membrane

[0490] [Chemistry 77]

[0491]

[0492] Under nitrogen atmosphere, add 10.0 g of compound (B8), 26.7 g of potassium carbonate and 130 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 68.0 g of the modifying agent (C7) and 200 g of DMF, which are pre-mixed and homogenized, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 500 g of MIBK and 400 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 170 g of THF to the residue, and after a uniform solution is obtained, add 1000 g of methanol dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 300 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain a compound (A15) for organic membranes.

[0493] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0494] (A15): Mw=2,450, Mw / Mn=1.02

[0495] (Synthesis Example 16)

[0496] Synthesis of Compound (A16) for Organic Membrane

[0497] [Chemistry 78]

[0498]

[0499] Under nitrogen atmosphere, add 10.0 g of compound (B8), 26.7 g of potassium carbonate and 130 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 66.0 g of the modifying agent (C8) and 200 g of DMF, which are pre-mixed and homogenized, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 500 g of MIBK and 400 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% aqueous nitric acid solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 170 g of THF to the residue, and after a uniform solution is obtained, add 1000 g of methanol dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 300 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A16) for organic membrane.

[0500] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0501] (A16): Mw=2,380, Mw / Mn=1.03

[0502] (Synthesis Example 17)

[0503] Synthesis of Compound (A17) for Organic Membrane

[0504] [Chemistry 79]

[0505]

[0506] Under nitrogen atmosphere, add 10.0 g of compound (B9), 19.7 g of potassium carbonate and 90 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop the solution obtained by pre-mixing and homogenizing the modifying agent (C2) 30.9 g and 90 g of DMF, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 200 g of MIBK and 200 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 100 g of 3.0% nitric acid aqueous solution and 5 times with 100 g of pure water, and dry the organic layer under reduced pressure. Add 90 g of THF to the residue, and after it becomes a uniform solution, add dropwise to 400 g of hexane to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 100 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A17) for organic membrane.

[0507] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0508] (A17): Mw=1,730, Mw / Mn=1.01

[0509] (Synthesis Example 18)

[0510] Synthesis of Compound (A18) for Organic Membrane

[0511] [Chemistry 80]

[0512]

[0513] Under nitrogen atmosphere, add 10.0 g of compound (B9), 19.7 g of potassium carbonate and 90 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop the solution obtained by pre-mixing and homogenizing the modifying agent (C5) 34.4 g and DMF 100 g, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 200 g of MIBK and 200 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 100 g of 3.0% nitric acid aqueous solution and 5 times with 100 g of pure water, and dry the organic layer under reduced pressure. Add 100 g of THF to the residue, and after it becomes a uniform solution, add 400 g of methanol dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 100 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain compound (A18) for organic membrane.

[0514] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0515] (A18): Mw=1,880, Mw / Mn=1.02

[0516] (Synthesis Example 19)

[0517] Synthesis of Compound (A19) for Organic Membrane

[0518] [Chemistry 81]

[0519]

[0520] Under nitrogen atmosphere, add 10.0 g of compound (B10), 37.3 g of potassium carbonate and 150 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 57.2 g of the modifying agent (C3) and 170 g of DMF, which are pre-mixed and homogenized to obtain a solution, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 400 g of MIBK and 400 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 140 g of THF to the residue, and after a uniform solution is obtained, add 600 g of hexane dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 200 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain a compound (A19) for organic membranes.

[0521] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0522] (A19): Mw=2,050, Mw / Mn=1.03

[0523] (Synthesis Example 20)

[0524] Synthesis of Compound (A20) for Organic Membrane

[0525] [Chemistry 82]

[0526]

[0527] Under nitrogen atmosphere, add 10.0 g of compound (B10), 37.3 g of potassium carbonate, and 150 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly dropwise add a solution obtained by pre-mixing and homogenizing 65.3 g of the modifying agent (C5) and 200 g of DMF, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 500 g of MIBK (methyl isobutyl ketone) and 500 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 160 g of THF to the residue, and after a uniform solution is obtained, add dropwise 1,000 g of methanol to crystallize. The crystals that have been crystallized are separated by filtration, washed twice with 300 g of methanol, and recovered. The recovered crystals were vacuum dried at 70° C. to obtain a compound for an organic film (A20).

[0528] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0529] (A20): Mw=2,460, Mw / Mn=1.02

[0530] (Synthesis Example 21)

[0531] Synthesis of Compound (A21) for Organic Membrane

[0532] [Chemistry 83]

[0533]

[0534] Under nitrogen atmosphere, add 10.0 g of compound (B11), 27.2 g of potassium carbonate and 110 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop the solution obtained by pre-mixing and homogenizing 42.7 g of the modifying agent (C2) and 130 g of DMF, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 400 g of MIBK and 400 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 110 g of THF to the residue, and after it becomes a uniform solution, add 500 g of hexane dropwise to crystallize. The crystallized crystals are separated by filtration, washed twice with 200 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain the compound (A21) for organic membrane.

[0535] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0536] (A21): Mw=2,310, Mw / Mn=1.03

[0537] (Synthesis Example 22)

[0538] Synthesis of Compound (A22) for Organic Membrane

[0539] [Chemistry 84]

[0540]

[0541] Under nitrogen atmosphere, add 10.0 g of compound (B11), 27.2 g of potassium carbonate and 110 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 54.9 g of the modifying agent (C6) and 160 g of DMF, which are pre-mixed and homogenized, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 500 g of MIBK and 500 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 140 g of THF to the residue, and after a uniform solution is obtained, add 600 g of methanol dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 200 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain a compound (A22) for organic membranes.

[0542] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0543] (A22): Mw=2,940, Mw / Mn=1.02

[0544] (Synthesis Example 23)

[0545] Synthesis of Compound (A23) for Organic Membrane

[0546] [Chemistry 85]

[0547]

[0548] Under nitrogen atmosphere, add 10.0 g of compound (B12), 22.3 g of potassium carbonate and 100 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop 34.3 g of the modifying agent (C3) and 110 g of DMF, which are pre-mixed and homogenized to obtain a solution, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 400 g of MIBK and 300 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 100 g of THF to the residue, and after it becomes a uniform solution, add 500 g of hexane dropwise to crystallize the crystals. The crystallized crystals are separated by filtration, washed twice with 200 g of hexane and recovered. The recovered crystals are vacuum dried at 70°C to obtain a compound (A23) for organic membranes.

[0549] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0550] (A23): Mw=2,360, Mw / Mn=1.03

[0551] (Synthesis Example 24)

[0552] Synthesis of Compound (A24) for Organic Membrane

[0553] [Chemistry 86]

[0554]

[0555] Under nitrogen atmosphere, add 10.0 g of compound (B12), 22.3 g of potassium carbonate, and 100 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop the solution obtained by pre-mixing and homogenizing 39.1 g of the modifying agent (C5) and 120 g of DMF, and react at an internal temperature of 50°C for 24 hours. After cooling to room temperature, add 400 g of MIBK and 300 g of pure water. After a uniform solution is obtained, remove the aqueous layer. In addition, wash the organic layer twice with 150 g of 3.0% nitric acid aqueous solution and 5 times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 110 g of THF to the residue, and after it becomes a uniform solution, add dropwise 500 g of methanol to crystallize. The crystallized crystals are separated by filtration, washed twice with 200 g of methanol and recovered. The recovered crystals are vacuum dried at 70°C to obtain the compound (A24) for organic membrane.

[0556] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0557] (A24): Mw=2,840, Mw / Mn=1.04

[0558] (Synthesis Example 25)

[0559] Synthesis of Compound (A25) for Organic Membrane

[0560] [Chemistry 87]

[0561]

[0562] Under nitrogen atmosphere, add 10.0 g of compound (B11), 27.2 g of potassium carbonate, and 110 g of DMF to prepare a uniform dispersion at an internal temperature of 50°C. Slowly drop a solution obtained by premixing and homogenizing 16.7 g of a modifying agent (C3) and 50 g of DMF, and react at an internal temperature of 50°C for 8 hours. Slowly drop a solution obtained by premixing and homogenizing 23.8 g of a modifying agent (C5) and 75 g of DMF, and react for another 16 hours. After cooling to room temperature, add 500 g of MIBK (methyl isobutyl ketone) and 500 g of pure water, and remove the aqueous layer after a uniform solution is obtained. In addition, wash the organic layer twice with 150 g of a 3.0% nitric acid aqueous solution and five times with 150 g of pure water, and dry the organic layer under reduced pressure. Add 100 g of THF to the residue, and after a uniform solution is obtained, drop 500 g of hexane to crystallize. The crystals obtained by crystallization were separated by filtration, washed twice with 200 g of hexane and recovered. The recovered crystals were vacuum dried at 70°C to obtain a compound for organic membrane (A25).

[0563] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0564] (A25): Mw=1,830, Mw / Mn=1.09

[0565] (Comparative Synthesis Example 1)

[0566] Synthesis of Compound (R1) for Comparative Example

[0567] [Chemistry 88]

[0568]

[0569] Under nitrogen atmosphere, 13.7 g of m-ethynylaniline, 13.3 g of triethylamine and 150 g of THF were stirred at room temperature to form a uniform solution. After slowly dropping THF10 g and 10.0 g of cyanuric chloride to form a uniform solution, the mixture was reacted under circulation for 5 hours. After cooling to room temperature, 150 g of methyl isobutyl ketone and 100 g of pure water were added to form a uniform solution, and the aqueous layer was removed. The organic layer was then washed twice with 50 g of 3.0% nitric acid aqueous solution and 5 times with 50 g of pure water, and the organic layer was dried under reduced pressure. 60 g of THF was added to the residue to form a uniform solution, and then crystallized with 200 g of hexane. The crystallized crystals were separated by filtration, washed twice with 100 g of hexane and recovered. The recovered crystals were vacuum dried at 70°C to obtain the comparative example compound (R1).

[0570] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0571] (R1): Mw=430, Mw / Mn=1.01

[0572] (Comparative Synthesis Example 2)

[0573] Synthesis of Compound (R2) for Comparative Example

[0574] [Chemistry 89]

[0575]

[0576] Under nitrogen atmosphere, 13.7 g of m-ethynylaniline, 13.3 g of triethylamine and 150 g of THF were stirred in an ice bath to form a uniform solution. 10 g of THF and 10.0 g of trimesoyl chloride were slowly added dropwise to form a uniform solution, and the mixture was reacted in an ice bath for 1 hour and at room temperature for 3 hours. After cooling to room temperature, 150 g of methyl isobutyl ketone and 100 g of pure water were added to form a uniform solution, and the aqueous layer was removed. The organic layer was then washed twice with 50 g of 3.0% nitric acid aqueous solution and 5 times with 50 g of pure water, and the organic layer was dried under reduced pressure. 60 g of THF was added to the residue to form a uniform solution, and then crystallized with 200 g of methanol. The crystallized crystals were separated by filtration, washed twice with 100 g of methanol and recovered. The recovered crystals were vacuum dried at 70°C to obtain the comparative example compound (R2).

[0577] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0578] (R2): Mw=520, Mw / Mn=1.01

[0579] (Comparative Synthesis 3)

[0580] Synthesis of Compound (R3) for Comparative Example

[0581] [Chemistry 90]

[0582]

[0583] Under a nitrogen environment, 10.00 g of the comparative example compound raw material (D1), 4.76 g of potassium carbonate, and 50 g of DMF were prepared into a uniform dispersion at an internal temperature of 50°C. 3.72 g of propargyl bromide was slowly added dropwise, and the reaction was carried out at an internal temperature of 50°C for 16 hours. After cooling to room temperature, 100 g of methyl isobutyl ketone and 50 g of pure water were added, and after a uniform solution was formed, the aqueous layer was removed. In addition, the organic layer was washed twice with 30 g of 3.0% nitric acid aqueous solution and 5 times with 30 g of pure water, and the organic layer was dried under reduced pressure. 30 g of THF was added to the residue, and crystallized with 100 g of methanol. The crystallized crystals were separated by filtration, washed twice with 60 g of methanol and recovered. The recovered crystals were vacuum dried at 70°C to obtain the comparative example compound (R3).

[0584] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.

[0585] (R3): Mw=960, Mw / Mn=1.07

[0586] Tables 1 to 4 show the results of Mw and Mw / Mn of the organic film compounds (A1) to (A25) used in Examples and the comparative example compounds (R1) to (R3).

[0587] [Table 1]

[0588]

[0589] [Table 2]

[0590]

[0591] [Table 3]

[0592]

[0593] [Table 4]

[0594]

[0595] [Preparation of organic film-forming materials (UDL-1 to 29, comparative UDL-1 to 3)]

[0596] The above-mentioned organic film-forming compounds (A1) to (A25), comparative example compounds (R1) to (R3), (S1) 1,6-diacetoxyhexane as a high boiling point solvent: boiling point 260°C, (S2) tripropylene glycol monomethyl ether: boiling point 242°C, propylene glycol monomethyl ether acetate (PGMEA) containing 0.1% by mass of PF-6320 (manufactured by Omnova) were dissolved in the proportions shown in Table 5, and filtered with a 0.1μm fluororesin filter to prepare organic film-forming materials (UDL-1 to 29, comparative UDL-1 to 3), respectively.

[0597] [Table 5]

[0598]

[0599] [Example 1 Solvent Resistance Measurement (Examples 1-1 to 1-29, Comparative Examples 1-1 to 1-3)]

[0600] The UDL-1 to 29 and comparative UDL-1 to 3 prepared above were coated on a silicon substrate, and baked in the air at the temperature shown in Table 6 for 60 seconds, and the film thickness was measured. PGMEA solvent was dispensed on it, left for 30 seconds and spin-dried, and baked at 100°C for 60 seconds to evaporate PGMEA, and the film thickness before and after PGMEA treatment was measured. The film thickness a after film formation and the film thickness b after PGMEA treatment were used to calculate the residual film rate. The results are shown in Table 6.

[0601] [Table 6]

[0602]

[0603]

[0604] As shown in Table 6, the organic membranes (Examples 1-1 to 1-29) using the compound for an organic membrane of the present invention had a residual film rate of 99.5% or more after PGMEA treatment, indicating that a crosslinking reaction occurred by heat treatment and sufficient solvent resistance was exhibited.

[0605] [Example 2 Evaluation of heat resistance characteristics (Examples 2-1 to 2-29, Comparative Examples 2-1 to 2-3)]

[0606] The above-mentioned organic film forming materials (UDL-1 to 29, comparative UDL-1 to 3) were coated on a silicon substrate, respectively, and baked in the air at the temperature described in Table 7 for 60 seconds to form a 200 nm coating film, and the film thickness a was measured. The substrate was further fired at 400°C for 20 minutes under a nitrogen flow with an oxygen concentration of 0.2% or less, and the film thickness b was measured. The residual film rate was calculated using the film thickness a after baking and the film thickness b after firing. These results are shown in Table 7.

[0607] [Table 7]

[0608]

[0609]

[0610] As shown in Table 7, the organic films (Examples 2-1 to 2-29) using the organic film compound of the present invention have a film thickness reduction of less than 5% after being fired at 400°C for a long time, which shows that the organic film forming material of the present invention has excellent heat resistance. In particular, it is known that the structure represented by the above general formula (2) is n 2 = 1 and a propargyl group or an ethynyl group introduced therein, the residual film rate was maintained at 98% or more and the heat resistance was particularly excellent.

[0611] [Evaluation of landfill characteristics in Example 3 (Examples 3-1 to 3-29, Comparative Examples 3-1 to 3-3)]

[0612] The organic film-forming materials (UDL-1 to 29, comparative UDL-1 to 3) prepared above were coated on SiO2 films having a dense hole pattern (hole diameter 0.16 μm, hole depth 0.50 μm, and center-to-center distance between two adjacent holes 0.32 μm). 2 The organic film was formed on the wafer substrate by firing in the atmosphere at the temperature listed in Table 8 for 60 seconds. The substrate used was a substrate having Figure 2 The dense hole pattern shown in (G) (overhead view) and (H) (cross-sectional view) of the base substrate 7 (SiO 2 Wafer substrate). The film forming property and filling property of each obtained wafer substrate were evaluated.

[0613] Regarding the film forming property, when no dewetting was observed on each of the obtained wafers by visual observation, it was rated as good, and when dewetting was observed, it was rated as poor. Regarding the filling property, the cross-sectional shape was observed using a scanning electron microscope (SEM) to confirm whether the pores were filled with the organic film 8 without pores (voids) inside. The results are shown in Table 8. In this evaluation, when an organic film material with good filling property was used, in this evaluation, if Figure 2 As shown in (I), the pores were filled with the organic film without voids, which was evaluated as good. When an organic film material with poor filling properties was used, voids occurred in the pores, which was evaluated as poor.

[0614] [Table 8]

[0615]

[0616]

[0617] As shown in Examples 3-1 to 3-29 in Table 8, when the organic film-forming compound of the present invention is used, all organic film-forming materials can form a densely pore-patterned SiO2 layer. 2 Film formation on the wafer substrate can fill the hole pattern without pores, which shows that the filling property is excellent. Moreover, Comparative Example 3-3 can also form a film on the above substrate and fill the hole pattern without pores. On the other hand, Comparative Example 3-1 does not have an amide structure, and Comparative Example 3-2 is a structure without an alkylene group between the amide structure and the aromatic ring, so the film forming property is not good, and poor film formation (dewetting) occurs on the substrate. It is believed that the structures of the compounds used in these organic film forming materials are all high in thermal fluidity but do not have an amide structure, so the adhesion with the substrate is weak, or there is no alkylene group between the amide structure and the aromatic ring, so the crystallinity is high, and thus the cohesion is strong, resulting in the above-mentioned poor film formation.

[0618] [Example 4 Evaluation of Flattening Characteristics (Examples 4-1 to 4-29, Comparative Examples 4-1 to 4-3)]

[0619] The organic film-forming materials (UDL-1 to 29, comparative UDL-1 to 3) prepared above were coated on Figure 3 Base substrate 9 (SiO 2 Wafer substrate) was baked in the atmosphere at the temperature described in Table 9 for 60 seconds, and the Alpha-Step D-600 (contact profiler) manufactured by KLA-TENCOR was used to observe the Figure 3The height difference (delta 10) of the organic film 10 having the groove part and the non-groove part shown in (K). The results are shown in Table 9. In this evaluation, the height difference is evaluated as S when it is less than 60nm, A when it is greater than 60nm and less than 80nm, B when it is greater than 80nm and less than 100nm, C when it is greater than 100nm and less than 115nm, and D when it is greater than 115nm. In this evaluation, the smaller the height difference, the better the planarization characteristics. In addition, in this evaluation, the groove pattern with a depth of 0.115μm is planarized using an organic film forming material with a normal film thickness of about 0.2μm, which is a strict evaluation condition for evaluating the quality of the planarization characteristics.

[0620] [Table 9]

[0621]

[0622]

[0623] As shown in Examples 4-1 to 4-29 of Table 9, when the organic film compound of the present invention is used, all organic film forming materials have excellent film forming properties compared to Comparative Examples 4-1 to 4-2, and compared to Comparative Example 4-3, the height difference of the organic film between the trench portion and the non-trench portion is small and the flattening property is excellent. In particular, the compound having an ether bond and the compound having a tertiary amide structure as represented by the aforementioned general formula (8) have excellent thermal fluidity, thereby improving the flattening property, and the organic film material having the characteristics of both has the best flattening property. In addition, the organic film forming material containing a high boiling point solvent has better flattening properties than the organic film material not containing a high boiling point solvent because of the thermal fluidity (Examples 4-26 to 4-29). On the other hand, in Comparative Examples 4-1 and 4-2, poor film formation (dewetting) occurred on the aforementioned giant isolated trench pattern substrate, which is believed to be due to the above-mentioned SiO with dense hole pattern. 2 The reason why the film formation failure occurred on the wafer substrate was the same. In addition, the compound of Comparative Example 4-3 lacked thermal fluidity, resulting in low planarization characteristics.

[0624] [Example 5 Adhesion Test (Examples 5-1 to 5-29, Comparative Examples 5-1 to 5-3)]

[0625] The above-mentioned organic film forming materials (UDL-1 to 29, comparative UDL-1 to 3) were coated on SiO 2On the wafer substrate, a hot plate is used to bake at the temperature described in Table 10 for 60 seconds in the atmosphere to form an organic film with a thickness of 200nm. The wafer with the organic film is cut into 1×1cm squares, and an aluminum pin with epoxy adhesive is installed on the cut wafer using a special fixture. Then, an oven is used to heat at 150℃ for 1 hour to bond the aluminum pin to the substrate. After cooling to room temperature, the initial adhesion is evaluated by resistance using a thin film adhesion strength measuring device (Sebastian Five-A).

[0626] Figure 4 This is a diagram illustrating the adhesion measurement method. Figure 4 11 represents the silicon wafer (substrate), 12 represents the hardened film, 14 represents the aluminum pin with the adhesive, 13 represents the support table, 15 represents the gripping point, and 16 represents the stretching direction. The adhesion is the average value of the 12-point measurement. The higher the value, the higher the adhesion of the organic film to the substrate. The adhesion is evaluated by comparing the obtained values. The results are shown in Table 10.

[0627] [Table 10]

[0628]

[0629]

[0630] As shown in Examples 5-1 to 5-29 of Table 10, the organic film forming material using the organic film compound having an amide structure of the present invention exhibits higher adhesion than Comparative Examples 5-1 and 5-3. In addition, the compound used in Comparative Example ULD-2, which exhibited poor film formation in Comparative Examples 3-2 and 4-2, has an amide structure, and as shown in Comparative Example 5-2, has the same adhesion as the organic film compound of the present invention. These results also indicate that the organic film forming material of the present invention has excellent thermal fluidity, and exhibits excellent film-forming properties due to the high degree of adhesion obtained by the amide structure and the relaxing effect of crystallinity obtained by the alkylene group between the amide structure and the aromatic ring.

[0631] [Example 6 Pattern Formation Test (Examples 6-1 to 6-29, Comparative Example 6-1)]

[0632] The above-mentioned organic film forming materials (UDL-1 to 29, comparative UDL-3) were applied on Figure 3 Base substrate 9 (SiO 2Wafer substrate), and fired in the atmosphere on a bare Si substrate in a manner such that the film thickness becomes 200nm under the conditions shown in Table 14 to form an organic film (resist lower film). A silicon-containing resist intermediate film material (SOG-1) was coated thereon, and baked at 220°C for 60 seconds to form a resist intermediate film with a film thickness of 35nm, and a resist upper film material (SL resist for ArF) was coated thereon, and baked at 105°C for 60 seconds to form a resist upper film with a film thickness of 100nm. A wet protection film (TC-1) was coated on the resist upper film, and baked at 90°C for 60 seconds to form a protection film with a film thickness of 50nm. In addition, for Comparative Examples 4-1 and 4-2, Comparative UDL-1 to 2, in which poor film formation occurred, the pattern formation test could not be carried out.

[0633] As the resist upper layer film material (SL resist for ArF), a polymer (RP1), an acid generator (PAG1), and a basic compound (Amine1) are dissolved in a solvent containing 0.1 mass % of FC-430 (manufactured by Sumitomo 3M Co., Ltd.) according to the proportions in Table 11, and the mixture is filtered through a 0.1 μm fluororesin filter to prepare the material.

[0634] [Table 11]

[0635]

[0636] The structural formulas of the polymer (RP1), the acid generator (PAG1), and the basic compound (Amine1) used are shown below.

[0637] [Chemistry 91]

[0638]

[0639] The wet protective film material (TC-1) was prepared by dissolving the protective film polymer (PP1) in an organic solvent according to the ratio shown in Table 12 and filtering the solution with a 0.1 μm fluororesin filter.

[0640] [Table 12]

[0641]

[0642] The structural formula of the protective film polymer (PP1) used is shown below.

[0643] [Chemistry 92]

[0644]

[0645] As a silicon-containing anti-etching intermediate film material (SOG-1), a polymer represented by an ArF silicon-containing intermediate film polymer (SiP1) and a thermal cross-linking catalyst (CAT1) are dissolved in an organic solvent containing 0.1 mass % of FC-4430 (produced by Sumitomo 3M Co., Ltd.) in the proportions shown in Table 13, and the silicon-containing anti-etching intermediate film material (SOG-1) is prepared by filtering with a fluororesin filter having a pore size of 0.1 μm.

[0646] [Table 13]

[0647]

[0648] The structural formulas of the ArF silicon-containing intermediate film polymer (SiP1) and the crosslinking catalyst (CAT1) used are shown below.

[0649] [Chemistry 93]

[0650]

[0651] Secondly, exposure was performed while changing the exposure amount using an ArF immersion exposure device (manufactured by Nikon Co., Ltd.; NSR-S610C, NA1.30, σ0.98 / 0.65, 35 degree dipole s-polarized illumination, 6% half-step phase shift mask), and baked (PEB) was performed at 100°C for 60 seconds. The image was developed with a 2.38 mass % tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds, and a positive line and space pattern (resist upper film pattern) with a resist line width of 50nm to 30nm at a pitch of 100nm was obtained.

[0652] Next, the resist upper layer film pattern obtained by dry etching with the Tokyo Electron etching apparatus Telius was used as a mask to process the silicon-containing intermediate film (SOG-1 film), the organic film was processed using the SOG-1 film as a mask, and the SiO 2 Processing of wafer substrates.

[0653] The etching conditions are as follows.

[0654] Transfer conditions of the resist upper layer film pattern to the SOG-1 film.

[0655]

[0656] Transfer conditions of SOG-1 film to organic film.

[0657]

[0658] Organic film to SiO 2 Transfer conditions of wafer substrate.

[0659]

[0660]

[0661] The pattern cross-section was observed using an electron microscope (S-4700) manufactured by Hitachi, Ltd., and the shapes were compared and summarized in Table 14.

[0662] [Table 14]

[0663]

[0664]

[0665] As shown in Table 14, the organic film forming material of the present invention, as shown in the results of Examples 6-1 to 6-29, the resist upper film pattern was finally well transferred to the substrate, confirming that the organic film forming material of the present invention is suitable for use in micro-processing using a multilayer resist method. On the other hand, in Comparative Example 6-1, as shown in the results of Comparative Example 4-3, the height difference on the pattern substrate was large, and the focus was deviated during exposure, so the patterned shape of the resist upper film was defective, and a part of the pattern collapsed during pattern processing.

[0666] From the above, it can be seen that if the organic film compound of the present invention or the organic film forming material of the present invention containing the same has good film-forming properties and adhesion, and excellent filling / planarization characteristics, it is extremely useful as an organic film (resist underlayer film) used in a multilayer resist method. Moreover, if the pattern forming method of the present invention is used, even if the processed body is a substrate with a height difference, a fine pattern can still be formed with high precision.

[0667] This specification includes the following aspects.

[0668] [1]: An organic film forming material, characterized by comprising an organic film forming compound represented by the following general formula (1) and an organic solvent,

[0669] [Chemistry 94]

[0670]

[0671] Where W 1 For n containing aromatic rings 1 valent organic group, L is a substituent on the aromatic ring and is represented by the following general formula (2): 1 , L 2 or both thereof, let the total number of substituents L on the aromatic ring be n 1 , L 1 The number of x, L 2 When the number of is y, it satisfies x+y=n 1 , 2≤n 1≤8, 0≤y≤8, 0≤x≤8,

[0672] [Chemistry 95]

[0673]

[0674] Where n 2 represents an integer from 1 to 3, R 1 is any of the following formula (3), R 2 is any of the following general formula (4),

[0675] [Chemistry 96]

[0676]

[0677] [Chemistry 97]

[0678]

[0679] In the formula, R 3 is any of the following formula (5), n 3 Indicates 0 or 1, n 4 Indicates 1 or 2.

[0680] [Chemistry 98]

[0681]

[0682] [2]: The organic film forming material according to [1], wherein L constituting the substituent L on the aromatic ring of the organic film forming compound represented by the general formula (1) is 1 , L 2 , expressed by the following general formula (6),

[0683] [Chemistry 99]

[0684]

[0685] In the formula, R 1 and R 2 Same as above.

[0686] [3]: The organic film forming material according to [1] or [2], wherein L constituting the substituent L on the aromatic ring of the organic film forming compound represented by the general formula (1) is 1 , L 2 R 1 , R 2 , is any one of the combinations represented by the following general formula (7),

[0687] [Chemical 100]

[0688]

[0689] In the formula, R 3 、n 4 Same as above.

[0690] [4]: The organic film forming material according to any one of [1] to [3], wherein the total number of substituents L on the aromatic ring of the organic film forming compound represented by the general formula (1) is n 1 Meets 3≤n 1 ≤6.

[0691] [5]: The organic film forming material according to any one of [1] to [4], wherein the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the organic film forming compound in terms of polystyrene obtained by gel permeation chromatography is 1.00≤Mw / Mn≤1.15.

[0692] [6]: The organic film forming material according to any one of [1] to [5], wherein the organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.

[0693] [7]: The organic film-forming material according to any one of [1] to [6], further comprising one or more of a surfactant and a plasticizer.

[0694] [8]: A pattern forming method is a method for forming a pattern on a workpiece, characterized by:

[0695] Forming an organic film on a workpiece using the organic film forming material described in any one of [1] to [7],

[0696] On the organic film, a silicon-containing resist intermediate film is formed using a silicon-containing resist intermediate film material.

[0697] A photoresist composition is used to form a resist upper film on the silicon-containing resist intermediate film.

[0698] forming a circuit pattern on the resist upper film,

[0699] The pattern is transferred to the silicon-containing resist intermediate film by etching using the patterned resist upper film as a mask.

[0700] The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film having the transferred pattern as a mask.

[0701] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0702] [9]: A pattern forming method is a method for forming a pattern on a workpiece, characterized by:

[0703] Forming an organic film on a workpiece using the organic film forming material described in any one of [1] to [7],

[0704] On the organic film, a silicon-containing resist intermediate film is formed using a silicon-containing resist intermediate film material.

[0705] forming an organic anti-reflective film (BARC) on the aforementioned silicon-containing resist intermediate film,

[0706] On the aforementioned BARC, a resist upper layer film is formed using a photoresist composition to form a 4-layer film structure.

[0707] forming a circuit pattern on the resist upper film,

[0708] The patterned resist upper film is used as a mask to transfer the pattern to the BARC and the silicon-containing resist intermediate film by etching.

[0709] The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film having the transferred pattern as a mask.

[0710] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0711]

[10] : A pattern forming method is a method for forming a pattern on a workpiece, characterized by:

[0712] Forming an organic film on a workpiece using the organic film forming material described in any one of [1] to [7],

[0713] On the organic film, an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film is formed.

[0714] On the inorganic hard mask intermediate film, a resist upper layer film is formed using a photoresist composition.

[0715] forming a circuit pattern on the resist upper film,

[0716] The pattern is transferred to the inorganic hard mask intermediate film by etching using the patterned resist upper film as a mask.

[0717] The inorganic hard mask intermediate film with the transferred pattern is used as a mask to transfer the pattern to the organic film by etching.

[0718] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0719]

[11] : A pattern forming method is a method for forming a pattern on a workpiece, characterized by:

[0720] Forming an organic film on a workpiece using the organic film forming material described in any one of [1] to [7],

[0721] On the organic film, an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film is formed.

[0722] On the inorganic hard mask intermediate film, an organic anti-reflection film (BARC) is formed.

[0723] On the aforementioned BARC, a resist upper layer film is formed using a photoresist composition to form a 4-layer film structure.

[0724] forming a circuit pattern on the resist upper film,

[0725] The patterned resist upper layer film is used as a mask to transfer the pattern to the BARC and the inorganic hard mask intermediate film by etching.

[0726] The inorganic hard mask intermediate film with the transferred pattern is used as a mask to transfer the pattern to the organic film by etching.

[0727] Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

[0728]

[12] : The pattern forming method according to

[10] or

[11] , wherein the inorganic hard mask intermediate film is formed by a CVD method or an ALD method.

[0729]

[13] : A pattern forming method as described in any one of [8] to

[12] , wherein the pattern forming method of the aforementioned resist upper layer film is a pattern forming method using optical lithography with a wavelength of not less than 10 nm and not more than 300 nm, direct drawing using an electron beam, nanoimprinting, or a combination of these.

[0730]

[14] : The pattern forming method according to any one of [8] to

[13] , wherein the developing method of the pattern forming method is alkali development or organic solvent development.

[0731]

[15] : A pattern forming method as described in any one of [8] to

[14] , wherein a semiconductor device substrate, or a semiconductor device substrate on which a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film is formed as the aforementioned processed body.

[0732]

[16] : The pattern forming method of

[15] uses silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, manganese, molybdenum, ruthenium or their alloys as the aforementioned metal.

[0733]

[17] : A compound for an organic film, characterized by being represented by the following general formula (1):

[0734] [Chemistry 101]

[0735]

[0736] Where W 1 For n containing aromatic rings 1 valent organic group, L is a substituent on the aromatic ring and is represented by the following general formula (2): 1 , L 2 or both thereof, let the total number of substituents L on the aromatic ring be n 1 , L 1 The number of x, L 2 When the number of is y, it satisfies x+y=n 1 , 2≤n 1 ≤8, 0≤y≤8, 0≤x≤8,

[0737] [Chemistry 102]

[0738]

[0739] Where n 2 represents an integer from 1 to 3, R 1 is any of the following formula (3), R 2 is any of the following general formula (4),

[0740] [Chemistry 103]

[0741]

[0742] [Chemistry 104]

[0743]

[0744] In the formula, R 3 is any of the following formula (5), n 3 Indicates 0 or 1, n 4 Indicates 1 or 2.

[0745] [Chemistry 105]

[0746]

[0747] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative only, and any device having substantially the same configuration and exhibiting the same function and effect as the technical concept described in the claims of the present invention is included in the technical scope of the present invention.

[0748] Description of Reference Numerals

[0749] 1:Substrate

[0750] 2: Processing layer

[0751] 2a: Pattern formed on the processed layer

[0752] 3: Organic film

[0753] 3a: Organic film pattern

[0754] 4: Silicon-containing resist interlayer

[0755] 4a: Silicon-containing resist interlayer pattern

[0756] 5: Resist upper film

[0757] 5a: Resist upper film pattern

[0758] 6: Important part

[0759] 7: Base substrate with dense hole pattern

[0760] 8: Organic film

[0761] 9: Base substrate with large isolated trench patterns

[0762] 10: Organic film

[0763] delta 10: The difference in film thickness between the trench and non-trench parts of the organic film

[0764] 11: Silicon Wafer

[0765] 12: Hardened film

[0766] 13: Support Desk

[0767] 14: Aluminum pin with adhesive

[0768] 15: Grab

[0769] 16: stretching direction

Claims

1. An organic film-forming material, characterized in that Containing an organic film-forming compound represented by the following general formula (1) and an organic solvent, In the formula, W1 is an n1-valent organic group containing an aromatic ring, L is a substituent on the aromatic ring and is L1, L2 or both of them represented by the following general formula (2), and when the total number of substituents L on the aromatic ring is n1, the number of L1 is x, and the number of L2 is y, the relationship x+y=n1, 2≤n1≤8, 0≤y≤8, 0≤x≤8 is satisfied, In the formula, n2 represents an integer of 1 to 3, R1 is any one of the following formula (3), and R2 is any one of the following general formula (4), In the formula, R3 is any one of the following formula (5), n3 represents 0 or 1, n4 represents 1 or 2, 2. The organic film-forming material according to claim 1, wherein L1 and L2 constituting the substituents L on the aromatic ring of the organic film compound represented by the general formula (1) are represented by the following general formula (6): In the formula, R1 and R2 are the same as described above.

3. The organic film-forming material according to claim 1, wherein R1 and R2 in the substituents L1 and L2 on the aromatic ring of the organic film compound represented by the general formula (1) are any combination represented by the following general formula (7): In the formula, R3 and n4 are the same as described above.

4. The organic film-forming material according to claim 1, wherein The total number n1 of substituents L on the aromatic ring of the organic film compound represented by the general formula (1) satisfies 3≤n1≤6.

5. The organic film-forming material according to claim 1, wherein The ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn in terms of polystyrene obtained by gel permeation chromatography of the compound for an organic membrane is 1.00≤Mw / Mn≤1.

15.

6. The organic film-forming material according to claim 1, wherein The organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180° C. and one or more organic solvents having a boiling point of 180° C. or higher.

7. The organic film-forming material according to claim 1, further comprising at least one of a surfactant and a plasticizer.

8. A method for forming a pattern on a workpiece, characterized by: : Forming an organic film on a workpiece using the organic film forming material according to any one of claims 1 to 7, On the organic film, a silicon-containing resist intermediate film is formed using a silicon-containing resist intermediate film material. A resist upper layer film is formed on the silicon-containing resist intermediate film using a photoresist composition. A circuit pattern is formed on the upper layer of the resist. The patterned resist upper layer film is used as a mask to transfer the pattern to the silicon-containing resist intermediate film by etching. The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask. Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

9. A method for forming a pattern on a workpiece, characterized in that : Forming an organic film on a workpiece using the organic film forming material according to any one of claims 1 to 7, On the organic film, a silicon-containing resist intermediate film is formed using a silicon-containing resist intermediate film material. forming an organic anti-reflective film (BARC) on the silicon-containing resist intermediate film, On the BARC, a resist upper layer film is formed using a photoresist composition to form a 4-layer film structure. A circuit pattern is formed on the upper layer of the resist. The patterned resist upper film is used as a mask to transfer the pattern to the BARC and the silicon-containing resist intermediate film by etching. The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask. Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

10. A method for forming a pattern on a workpiece, characterized by: : Forming an organic film on a workpiece using the organic film forming material according to any one of claims 1 to 7, On the organic film, an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film is formed, On the inorganic hard mask intermediate film, a resist upper layer film is formed using a photoresist composition. A circuit pattern is formed on the upper layer of the resist. The patterned resist upper layer film is used as a mask, and the pattern is transferred to the inorganic hard mask intermediate film by etching. The inorganic hard mask intermediate film with the transferred pattern is used as a mask to transfer the pattern to the organic film by etching. Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

11. A method for forming a pattern on a workpiece, characterized by: : Forming an organic film on a workpiece using the organic film forming material according to any one of claims 1 to 7, On the organic film, an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film is formed, On top of the inorganic hard mask intermediate film, an organic anti-reflection film (BARC) is formed. On the BARC, a resist upper layer film is formed using a photoresist composition to form a 4-layer film structure. A circuit pattern is formed on the upper layer of the resist. The patterned resist upper layer film is used as a mask to transfer the pattern to the BARC and the inorganic hard mask intermediate film by etching. The inorganic hard mask intermediate film with the transferred pattern is used as a mask to transfer the pattern to the organic film by etching. Furthermore, the object to be processed is etched using the organic film to which the pattern has been transferred as a mask, thereby forming a pattern on the object to be processed.

12. The pattern forming method according to claim 10, wherein: The inorganic hard mask intermediate film is formed by a CVD method or an ALD method.

13. The pattern forming method according to claim 8, wherein: The patterning method of the resist upper layer film is a patterning method using optical lithography with a wavelength of 10 nm to 300 nm, direct writing using an electron beam, nanoimprinting, or a combination thereof.

14. The pattern forming method according to claim 8, wherein: The developing method of the pattern forming method is alkali development or organic solvent development.

15. The pattern forming method according to claim 8 uses a semiconductor device substrate, or a semiconductor device substrate on which any of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film is formed as the processed body.

16. The pattern forming method according to claim 15, wherein the metal is silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, manganese, molybdenum, ruthenium or an alloy thereof.

17. A compound for an organic film, characterized by being represented by the following general formula (1): In the formula, W1 is an n1-valent organic group containing an aromatic ring, L is a substituent on the aromatic ring and is L1, L2 or both of them represented by the following general formula (2), and when the total number of substituents L on the aromatic ring is n1, the number of L1 is x, and the number of L2 is y, the relationship x+y=n1, 2≤n1≤8, 0≤y≤8, 0≤x≤8 is satisfied, In the formula, n2 represents an integer of 1 to 3, R1 is any one of the following formula (3), and R2 is any one of the following general formula (4), In the formula, R3 is any one of the following formula (5), n3 represents 0 or 1, n4 represents 1 or 2, 。