Cooling agent as well as preparation method and application thereof
Through mesoporous hollow silica nanosphere carrier and acid ionic liquid modification technology, sustained release cooling agents were prepared, solving the strong odor and irritation problems of existing cooling agents, and achieving a longer lasting coolness and aroma Coordinated, suitable for the cigarette industry.
Patent Information
- Application Number
- CN202410991430.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing cooling agents have problems such as strong odor, strong irritation, low reaction yield, large waste liquid emissions, high pollution and high energy consumption during use, which is difficult to meet the cigarette industry's demand for coolness and aroma.
Mesoporous hollow silica nanospheres are used as support, and the combination of mint glycerol ether cinnamon acetal and menthol, combined with acid ionic liquid modified polyvinyl pyrrolidone and catalyst were prepared to prepare a sustained-release cooling agent, using the emulsion method and Sol-gel reaction technology realizes the preparation of composite nanospheres and is coated with tannin to extend the release time.
It improves the durability and effect of the coolant, reduces the bad taste, significantly increases the coolness of the smoke, coordinates the tobacco fragrance, is suitable for the cigarette industry, and has broad application prospects.
Smart Images

Figure BDA0004958978150000021 
Figure BDA0004958978150000091 
Figure BDA0004958978150000141
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of food additives, and in particular to a cooling agent and a preparation method and application thereof. Background Art
[0002] Cooling agents are a general term for all chemical substances that can produce a cooling effect and are not very medicinal. The most common cooling agent is menthol (especially L-menthol), but due to its strong odor and strong irritation to the skin, mucous membranes and eyes, it is not suitable for large-scale use. Therefore, many scientists have synthesized and extracted a new generation of cooling agents.
[0003] Chinese patent document CN104642983A discloses a compound cooling agent composition and its preparation process, which is composed of the following components by mass percentage: ws-5 92.0-95.0% ws-3 5.0-8.0%; wherein ws-5 is ethyl acetate (N-ethyl-p-menthyl-3-carboxamide) ester, and ws-3 is N-ethyl-p-menthyl-3-carboxamide; the preparation method comprises the following steps: step 1: add water, glycine ethyl ester hydrochloride, sodium bicarbonate, and ethylamine into a three-necked flask, start stirring, fully dissolve, and control the temperature at 20-25°C; step 2: drop menthyl methyl chloride dissolved in n-hexane into the solution described in step 1, slowly drop, control the central temperature at 20-25°C, maintain the temperature after the dropwise addition, and continue stirring for 3-6 hours; step 3: after the reaction is completed, filter the reaction solution to obtain a white filter cake, wash the filter cake with water, filter again, vacuum dry the filter cake, then dissolve the filter cake with a small amount of solvent, and recrystallize with n-hexane to obtain the final product. However, the reaction yield is not high, the waste liquid discharge is large, the pollution is large, and the energy consumption is high. Summary of the invention
[0004] The purpose of the present invention is to provide a cooling agent and a preparation method and application thereof, which has a sustained release effect, prolongs its cooling time, improves its durability and effect, has a pure cooling taste, and has less unpleasant taste. It is suitable for the cigarette industry, can significantly increase the cooling feeling of smoke, coordinate the smoke aroma, and improve the aroma quality, and has broad application prospects.
[0005] The technical solution of the present invention is achieved in this way:
[0006] The present invention provides a method for preparing a cooling agent, comprising the following steps:
[0007] S1. Preparation of mesoporous hollow silica nanospheres: dissolving alkyl orthosilicate and an emulsifier in dichloromethane to obtain an organic phase; dissolving a porogen in water to obtain an aqueous phase; dropping the aqueous phase into the organic phase, emulsifying, adjusting the pH value of the solution, stirring the reaction, centrifuging, washing, drying, and calcining to obtain mesoporous hollow silica nanospheres;
[0008] S2. Preparation of Menthyl Glyceryl Ether Cinnamaldehyde: Menthyl Glyceryl Ether and Cinnamaldehyde are reacted in the presence of a catalyst to obtain Menthyl Glyceryl Ether Cinnamaldehyde; the structural formula is shown in Formula I:
[0009]
[0010] S3. Preparation of a composite cooling agent composition: The mint glyceryl ether cinnamic acetal and menthol were uniformly mixed to obtain a composite cooling agent composition;
[0011] S4. Immobilization: dissolving the composite cooling agent composition in ethanol, adding mesoporous hollow silica nanospheres, and evaporating the solvent to obtain composite nanospheres;
[0012] S5. Coating: adding the composite nanospheres into water, adding tannic acid and a catalyst, heating and stirring to react, centrifuging, washing, and drying to obtain a cooling agent.
[0013] As a further improvement of the present invention, the mass ratio of the alkyl orthosilicate, the emulsifier and the porogen in step S1 is 12-15:0.5-1:1-2, the emulsifier is selected from at least one of Span-20, Span-40, Span-60, Span-80 and Span-85, the porogen is hexadecyltrimethylammonium chloride or hexadecyltrimethylammonium bromide, the pH value of the adjusted solution is 9-10, the stirring reaction time is 10-12h, the calcination temperature is 450-550°C, and the time is 1-3h.
[0014] As a further improvement of the present invention, the molar ratio of the menthol ether to the cinnamaldehyde in step S2 is 1-1.1:1, the amount of the catalyst added is 0.5-1wt% of the total mass of the system, the reaction temperature is 70-80°C, the reaction time is 4-6h, and the preparation method of the catalyst is as follows:
[0015] T1. Preparation of mesoporous silica microspheres: dissolving alkyl orthosilicate and porogen in ethanol, adding ammonia solution to adjust the pH value of the solution, stirring the reaction, centrifuging, washing, drying, and calcining to obtain mesoporous silica microspheres;
[0016] T2. Preparation of polyvinyl pyrrolidone modified with acidic ionic liquid: adding polyvinyl pyrrolidone to toluene, adding 1,3-propane sultone and 1,4-butane sultone, heating and stirring to react, filtering, washing, drying, adding to ethyl acetate, adding tannic acid and a catalyst, stirring to react, filtering, washing, drying, and obtaining polyvinyl pyrrolidone modified with acidic ionic liquid;
[0017] T3. Immobilization: Add polyvinyl pyrrolidone modified with acidic ionic liquid into water, add mesoporous silica microspheres, evaporate the solvent at room temperature, and prepare composite microspheres;
[0018] T4. Preparation of catalyst: dissolve diethylaluminum chloride in n-hexane, add composite microspheres, stir to react, centrifuge, wash, and dry to obtain a catalyst.
[0019] As a further improvement of the present invention, the alkyl orthosilicate in step T1 is methyl orthosilicate or ethyl orthosilicate, the mass ratio of the alkyl orthosilicate and the porogen is 17-22:1-2, the porogen is hexadecyltrimethylammonium chloride or hexadecyltrimethylammonium bromide, the pH value of the adjusted solution is 8.5-9.5, the stirring reaction time is 7-10h, the calcination temperature is 450-550°C, and the time is 1-3h; the mass ratio of polyvinyl pyrrolidone, 1,3-propane sultone, 1,4-butane sultone, tannic acid and catalyst in step T2 is 10:3-4:2-3:7-10:0.5-1, the catalyst is a Tris-HCl solution with a pH of 8.5-9.5, the temperature of the heated stirring reaction is 75-85°C, the time is 20-24h, and the stirring reaction time is 3-5h.
[0020] As a further improvement of the present invention, the mass ratio of the acidic ionic liquid-modified polyvinyl pyrrolidone and the mesoporous silica microspheres in step T3 is 3-5:10; the mass ratio of diethylaluminum chloride and the composite microspheres in step T4 is 2-3:10, and the stirring reaction time is 0.5-1.5h.
[0021] As a further improvement of the present invention, the mass ratio of the menthyl ether cinnamic acetal to menthol in step S3 is 4-6:7-10.
[0022] As a further improvement of the present invention, the mass ratio of the composite cooling agent composition and the mesoporous hollow silica nanospheres in step S4 is 3-5:10.
[0023] As a further improvement of the present invention, the mass ratio of the composite nanospheres, tannic acid and catalyst in step S5 is 10:7-12:0.5-1, the temperature of the heating and stirring reaction is 35-45°C, the time is 2-4h, and the pH of the catalyst is Tris-HCl solution of 8.5-9.5.
[0024] The present invention further protects a cooling agent prepared by the above preparation method.
[0025] The present invention further protects the use of the above cooling agent in cigarettes.
[0026] The present invention has the following beneficial effects:
[0027] The invention allows menthol ether and cinnamaldehyde to react under the action of an acidic catalyst to obtain menthol ether cinnamaldehyde, which greatly improves the cooling effect. However, when used alone, it has a little pungent and tingling feeling. When used in combination with peppermint oil, the problem of bad taste is solved and the persistence and intensity of the cooling effect are greatly prolonged.
[0028] In the catalyst prepared by the present invention, polyvinyl polypyrrolidone is used as an adsorbent, and its adsorption effect enhances the adsorption of the catalyst to the reaction substrate, promotes the progress of the chemical reaction, and grafts ionic liquid on the surface, and further polymerizes and acidifies in acidic tannic acid to prepare polyvinyl pyrrolidone modified with acidic ionic liquid, which has good water solubility. After being dissolved in water, mesoporous silica microspheres are added, and since the microsphere surface has abundant pores, as the solvent water evaporates, the polyvinyl pyrrolidone modified with acidic ionic liquid is gradually adsorbed into the pores under the capillary force of the mesoporous pores, and gradually crystallizes in the pores, so as to be adsorbed in the mesoporous silica, and composite microspheres are prepared, and diethylaluminum chloride reacts with hydroxyl groups on the surface of the composite microspheres to remove ethane, so as to form a catalyst loaded with Lewis acid bonded by chemical bonds, which has high efficient catalytic ability for condensation reaction and still has high activity after repeated use.
[0029] The present invention adopts sol-gel reaction and emulsion method to prepare mesoporous hollow silica nanospheres, and stirs at room temperature to slowly volatilize ethanol. As the ethanol evaporates, the composite cooling agent composition is adsorbed into the hollow spheres under the capillary force of the mesoporous channels, and gradually crystallizes in the channels and the spheres, and is "concentrated" in the nanospheres. Then the composite nanospheres are added into water. Since the composite cooling agent composition is slightly soluble in water and is hardly released, after the surface is polymerized and coated with tannic acid, the semipermeable membrane characteristics of the polymer layer are utilized to achieve a slow release effect on the loaded composite cooling agent composition, thereby prolonging its cooling time and improving its durability and effect.
[0030] The cooling agent prepared by the invention has a sustained release effect, prolongs the cooling time, improves its durability and effect, has a pure cooling taste, and has less unpleasant taste. It is suitable for the cigarette industry, can significantly increase the cooling feeling of smoke, coordinate the smoke aroma, and improve the aroma quality, and has broad application prospects. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Preparation Example 1 Preparation of Catalyst
[0033] Here’s how:
[0034] T1. Preparation of mesoporous silica microspheres: 17 g of methyl orthosilicate and 1 g of hexadecyltrimethylammonium chloride were dissolved in 120 mL of ethanol, and an aqueous ammonia solution was added dropwise to adjust the solution pH to 8.5. The mixture was stirred for 7 h, centrifuged, washed, dried, and calcined at 450 ° C for 1 h to obtain mesoporous silica microspheres.
[0035] T2. Preparation of polyvinyl pyrrolidone modified with acidic ionic liquid: 10 g of polyvinyl pyrrolidone was added to 200 mL of toluene, 3 g of 1,3-propane sultone and 2 g of 1,4-butane sultone were added, the mixture was heated to 75°C, stirred for reaction for 20 h, filtered, washed, dried, added to ethyl acetate, 7 g of tannic acid and 0.5 g of catalyst were added, stirred for reaction at 40°C for 3 h, filtered, washed, dried, and polyvinyl pyrrolidone modified with acidic ionic liquid was obtained;
[0036] Tris-HCl solution of the catalyst with a pH of 8.5;
[0037] T3. Immobilization: Add 3 g of polyvinyl pyrrolidone modified with acidic ionic liquid to 50 mL of water, add 10 g of mesoporous silica microspheres, evaporate the solvent at room temperature to obtain composite microspheres;
[0038] T4. Preparation of catalyst: Dissolve 2 g of diethylaluminum chloride in 200 mL of n-hexane, add 10 g of composite microspheres, stir and react at 40°C for 0.5 h, centrifuge, wash, and dry to obtain the catalyst.
[0039] Preparation Example 2 Preparation of Catalyst
[0040] Here’s how:
[0041] T1. Preparation of mesoporous silica microspheres: 17 g of tetraethyl orthosilicate and 2 g of hexadecyltrimethylammonium bromide were dissolved in 120 mL of ethanol, and an aqueous ammonia solution was added dropwise to adjust the solution pH to 9.5. The mixture was stirred for 10 h, centrifuged, washed, dried, and calcined at 550 ° C for 3 h to obtain mesoporous silica microspheres.
[0042] T2. Preparation of polyvinyl pyrrolidone modified with acidic ionic liquid: 10 g of polyvinyl pyrrolidone was added to 200 mL of toluene, 4 g of 1,3-propane sultone and 3 g of 1,4-butane sultone were added, the mixture was heated to 85°C, stirred for reaction for 24 h, filtered, washed, dried, added to ethyl acetate, 10 g of tannic acid and 1 g of catalyst were added, stirred for reaction at 40°C for 5 h, filtered, washed, dried, and polyvinyl pyrrolidone modified with acidic ionic liquid was obtained;
[0043] The catalyst has a pH of 9.5 in a Tris-HCl solution;
[0044] T3. Immobilization: Add 5 g of polyvinyl pyrrolidone modified with acidic ionic liquid to 50 mL of water, add 10 g of mesoporous silica microspheres, evaporate the solvent at room temperature to obtain composite microspheres;
[0045] T4. Preparation of catalyst: Dissolve 3 g of diethylaluminum chloride in 200 mL of n-hexane, add 10 g of composite microspheres, stir and react at 40°C for 1.5 h, centrifuge, wash, and dry to obtain the catalyst.
[0046] Preparation Example 3 Preparation of Catalyst
[0047] Here’s how:
[0048] T1. Preparation of mesoporous silica microspheres: 20 g of tetraethyl orthosilicate and 1.5 g of hexadecyltrimethylammonium chloride were dissolved in 120 mL of ethanol, and an aqueous ammonia solution was added dropwise to adjust the solution pH to 9. The mixture was stirred for 8 h, centrifuged, washed, dried, and calcined at 500 ° C for 2 h to obtain mesoporous silica microspheres.
[0049] T2. Preparation of polyvinyl pyrrolidone modified with acidic ionic liquid: 10 g of polyvinyl pyrrolidone was added to 200 mL of toluene, 3.5 g of 1,3-propane sultone and 2.5 g of 1,4-butane sultone were added, the mixture was heated to 80°C, stirred for reaction for 22 h, filtered, washed, dried, added to ethyl acetate, 8.5 g of tannic acid and 0.7 g of catalyst were added, stirred for reaction at 40°C for 4 h, filtered, washed, dried, and polyvinyl pyrrolidone modified with acidic ionic liquid was obtained;
[0050] A Tris-HCl solution of the catalyst with a pH of 9;
[0051] T3. Immobilization: Add 4 g of polyvinyl pyrrolidone modified with acidic ionic liquid to 50 mL of water, add 10 g of mesoporous silica microspheres, evaporate the solvent at room temperature to obtain composite microspheres;
[0052] T4. Preparation of catalyst: Dissolve 2.6 g of diethylaluminum chloride in 200 mL of n-hexane, add 10 g of composite microspheres, stir and react at 40°C for 1 h, centrifuge, wash, and dry to obtain the catalyst.
[0053] Comparative Preparation Example 1
[0054] Compared with Preparation Example 3, the difference is that the porogen hexadecyltrimethylammonium chloride is not added in step T1.
[0055] The details are as follows:
[0056] T1. Preparation of silica microspheres: Dissolve 20 g of tetraethyl orthosilicate in 120 mL of ethanol, add dropwise an ammonia solution to adjust the solution pH to 9, stir and react for 8 h, centrifuge, wash, dry, and calcine at 500° C. for 2 h to obtain silica microspheres.
[0057] Comparative Preparation Example 2
[0058] Compared with Preparation Example 3, the difference is that tannic acid is not added in step T2.
[0059] The details are as follows:
[0060] T2. Preparation of ionic liquid modified polyvinyl pyrrolidone: Add 10 g of polyvinyl pyrrolidone into 200 mL of toluene, add 3.5 g of 1,3-propane sultone and 2.5 g of 1,4-butane sultone, heat to 80°C, stir to react for 22 hours, filter, wash, and dry to obtain ionic liquid modified polyvinyl pyrrolidone.
[0061] Comparative Preparation Example 3
[0062] Compared with Preparation Example 3, the difference is that step T4 is not performed.
[0063] The details are as follows:
[0064] T1. Preparation of mesoporous silica microspheres: 20 g of tetraethyl orthosilicate and 1.5 g of hexadecyltrimethylammonium chloride were dissolved in 120 mL of ethanol, and an aqueous ammonia solution was added dropwise to adjust the solution pH to 9. The mixture was stirred for 8 h, centrifuged, washed, dried, and calcined at 500 ° C for 2 h to obtain mesoporous silica microspheres.
[0065] T2. Preparation of polyvinyl pyrrolidone modified with acidic ionic liquid: 10 g of polyvinyl pyrrolidone was added to 200 mL of toluene, 3.5 g of 1,3-propane sultone and 2.5 g of 1,4-butane sultone were added, the mixture was heated to 80°C, stirred for reaction for 22 h, filtered, washed, dried, added to ethyl acetate, 8.5 g of tannic acid and 0.7 g of catalyst were added, stirred for reaction at 40°C for 4 h, filtered, washed, dried, and polyvinyl pyrrolidone modified with acidic ionic liquid was obtained;
[0066] A Tris-HCl solution of the catalyst with a pH of 9;
[0067] T3. Immobilization: Add 4 g of polyvinyl pyrrolidone modified with acidic ionic liquid into 50 mL of water, add 10 g of mesoporous silica microspheres, evaporate the solvent at room temperature to obtain composite microspheres, which are the catalyst.
[0068] Test Example 1
[0069] The catalysts prepared in Preparation Examples 1-3 of the present invention and Comparative Preparation Examples 1-3 were subjected to performance tests, and the specific surface area and pore volume parameters of the samples were measured using an American ASAP2460 fully automatic specific surface and porosity analyzer. The results are shown in Table 1.
[0070] Table 1
[0071] Group <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Total pore volume (cm 3 / g)]]> Preparation Example 1 615 0.61 Preparation Example 2 619 0.62 Preparation Example 3 622 0.64 Comparative Preparation Example 1 485 0.45 Comparative Preparation Example 2 597 0.57 Comparative Preparation Example 3 556 0.51
[0072] It can be seen from the above table that the catalysts prepared in Preparation Examples 1-3 of the present invention have larger specific surface areas and total pore volumes.
[0073] Example 1
[0074] This embodiment provides a method for preparing a cooling agent, comprising the following steps:
[0075] S1. Preparation of mesoporous hollow silica nanospheres: 12 g of tetraethyl orthosilicate and 0.5 g of Span-40 were dissolved in 500 mL of dichloromethane to obtain an organic phase; 1 g of hexadecyltrimethylammonium chloride was dissolved in 200 mL of water to obtain an aqueous phase; the aqueous phase was dripped into the organic phase, emulsified at 7000 r / min for 15 min, the pH value of the solution was adjusted to 9, the reaction was stirred for 10 h, centrifuged, washed, dried, and calcined at 450° C. for 1 h to obtain mesoporous hollow silica nanospheres;
[0076] S2. Preparation of Menthyl Glyceryl Ether Cinnamyl Acetal:
[0077] The synthetic route is as follows:
[0078]
[0079] 0.01 mol of menthol ether and 0.01 mol of cinnamaldehyde were added to 200 mL of N,N-dimethylformamide, and the catalyst prepared in Preparation Example 1 was added in an amount of 0.5 wt% of the total mass of the system. The mixture was stirred at 70° C. for 4 h to obtain menthol ether cinnamaldehyde. ESI-MS calculated value: C 22 H 33 O 3 (M+H)+345.24, found: 345.2, yield: 82.4%.
[0080] NMR results: 1 H NMR (300 MHz, CDCl 3)δ7.30 (d, J=6.4Hz, 2H), 7.22 (d, J=6.5Hz, 2H), 7.12 (m, 1H), 6.64 (d, J=4.2Hz, 1H), 6.21 (d, J=4.0Hz, 1H), 5.57 (d, 1H), 4.22 (m, 1H) , 3.86 (d, 2H), 3.50 (d, 2H), 2.77 (m, 1H), 1.83 (m, 1H), 1.75 (m, 1H), 1.62 (m, 1H), 1.55 (m, 2H), 1.42 (m, 4H), 1.07 (d, 3H), 1.01 (d, 6H).
[0081] S3. Preparation of a composite cooling agent composition: 0.4 g of menthol glyceryl ether cinnamic acetal and 0.7 g of menthol were stirred and mixed for 10 min to obtain a composite cooling agent composition;
[0082] S4. Immobilization: 0.3 g of the composite cooling agent composition was dissolved in 20 mL of ethanol, 1 g of mesoporous hollow silica nanospheres was added, and the solvent was evaporated to obtain composite nanospheres;
[0083] S5. Coating: Add 1 g of composite nanospheres to 50 mL of water, add 0.7 g of tannic acid and 0.05 g of catalyst, heat to 35°C, stir to react for 2 h, centrifuge, wash, and dry to obtain a cooling agent.
[0084] Example 2
[0085] This embodiment provides a method for preparing a cooling agent, comprising the following steps:
[0086] S1. Preparation of mesoporous hollow silica nanospheres: 15 g of tetraethyl orthosilicate and 1 g of Span-60 were dissolved in 500 mL of dichloromethane to obtain an organic phase; 2 g of hexadecyltrimethylammonium chloride was dissolved in 200 mL of water to obtain an aqueous phase; the aqueous phase was dripped into the organic phase, emulsified at 7000 r / min for 15 min, the pH value of the solution was adjusted to 10, the reaction was stirred for 12 h, centrifuged, washed, dried, and calcined at 550° C. for 3 h to obtain mesoporous hollow silica nanospheres;
[0087] S2. Preparation of menthol ether cinnamaldehyde: 0.011 mol menthol ether and 0.01 mol cinnamaldehyde were added to 200 mL N, N-dimethylformamide, and the catalyst prepared in Preparation Example 2 was added. The amount of the catalyst added was 1 wt% of the total mass of the system. The reaction was stirred at 80 ° C for 6 h to obtain menthol ether cinnamaldehyde in a yield of 81.1%;
[0088] S3. Preparation of a composite cooling agent composition: 0.6 g of menthol glyceryl ether cinnamic acetal and 1 g of menthol were stirred and mixed for 10 min to obtain a composite cooling agent composition;
[0089] S4. Immobilization: 0.5 g of the composite cooling agent composition was dissolved in 20 mL of ethanol, 1 g of mesoporous hollow silica nanospheres was added, and the solvent was evaporated to obtain composite nanospheres;
[0090] S5. Coating: Add 1 g of composite nanospheres to 50 mL of water, add 1.2 g of tannic acid and 0.1 g of catalyst, heat to 45°C, stir to react for 4 h, centrifuge, wash, and dry to obtain a cooling agent.
[0091] Example 3
[0092] This embodiment provides a method for preparing a cooling agent, comprising the following steps:
[0093] S1. Preparation of mesoporous hollow silica nanospheres: 13.5 g of tetraethyl orthosilicate and 0.7 g of Span-80 were dissolved in 500 mL of dichloromethane to obtain an organic phase; 1.5 g of hexadecyltrimethylammonium bromide was dissolved in 200 mL of water to obtain an aqueous phase; the aqueous phase was dripped into the organic phase, emulsified at 7000 r / min for 15 min, the pH value of the solution was adjusted to 9.5, the reaction was stirred for 11 h, centrifuged, washed, dried, and calcined at 500° C. for 2 h to obtain mesoporous hollow silica nanospheres;
[0094] S2. Preparation of menthol ether cinnamaldehyde: 0.0105 mol menthol ether and 0.01 mol cinnamaldehyde were added to 200 mL N, N-dimethylformamide, and the catalyst prepared in Preparation Example 3 was added. The amount of the catalyst added was 0.7 wt % of the total mass of the system. The reaction was stirred at 75 ° C for 5 h to obtain menthol ether cinnamaldehyde in a yield of 83.2%;
[0095] S3. Preparation of a composite cooling agent composition: 0.5 g of menthol glyceryl ether cinnamic acetal and 0.85 g of menthol were stirred and mixed for 10 min to obtain a composite cooling agent composition;
[0096] S4. Immobilization: 0.4 g of the composite cooling agent composition was dissolved in 20 mL of ethanol, 1 g of mesoporous hollow silica nanospheres was added, and the solvent was evaporated to obtain composite nanospheres;
[0097] S5. Coating: Add 1 g of composite nanospheres into 50 mL of water, add 1 g of tannic acid and 0.07 g of catalyst, heat to 40°C, stir to react for 3 h, centrifuge, wash, and dry to obtain a cooling agent.
[0098] Comparative Example 1
[0099] Compared with Example 3, the difference is that the catalyst is prepared by Comparative Preparation Example 1.
[0100] Comparative Example 2
[0101] Compared with Example 3, the difference is that the catalyst is prepared by Comparative Preparation Example 2.
[0102] Comparative Example 3
[0103] Compared with Example 3, the difference is that the catalyst is prepared by Comparative Preparation Example 3.
[0104] Comparative Example 4
[0105] Compared with Example 3, the difference is that cetyltrimethylammonium bromide is not added in step S1.
[0106] The details are as follows:
[0107] S1. Preparation of hollow silica nanospheres: 13.5 g of tetraethyl orthosilicate and 0.7 g of Span-80 were dissolved in 500 mL of dichloromethane to obtain an organic phase; 200 mL of water was dropped into the organic phase, emulsified at 7000 r / min for 15 min, the pH value of the solution was adjusted to 9.5, the reaction was stirred for 11 h, centrifuged, washed, dried, and calcined at 500°C for 2 h to obtain mesoporous hollow silica nanospheres.
[0108] Comparative Example 5
[0109] Compared with Example 3, the difference is that the composite cooling agent composition is replaced by single menthyl ether cinnamic acetal.
[0110] Comparative Example 6
[0111] Compared with Example 3, the difference is that the composite cooling agent composition is replaced by single menthol.
[0112] Comparative Example 7
[0113] Compared with Embodiment 3, the difference is that step S5 is not performed.
[0114] The details are as follows:
[0115] S1. Preparation of mesoporous hollow silica nanospheres: 13.5 g of tetraethyl orthosilicate and 0.7 g of Span-80 were dissolved in 500 mL of dichloromethane to obtain an organic phase; 1.5 g of hexadecyltrimethylammonium bromide was dissolved in 200 mL of water to obtain an aqueous phase; the aqueous phase was dripped into the organic phase, emulsified at 7000 r / min for 15 min, the pH value of the solution was adjusted to 9.5, the reaction was stirred for 11 h, centrifuged, washed, dried, and calcined at 500° C. for 2 h to obtain mesoporous hollow silica nanospheres;
[0116] S2. Preparation of menthol ether cinnamaldehyde: 0.0105 mol menthol ether and 0.01 mol cinnamaldehyde were added to 200 mL N, N-dimethylformamide, and the catalyst prepared in Preparation Example 3 was added. The amount of the catalyst added was 0.7 wt % of the total mass of the system. The reaction was stirred at 75 ° C for 5 h to obtain menthol ether cinnamaldehyde in a yield of 83.2%;
[0117] S3. Preparation of a composite cooling agent composition: 0.5 g of menthol glyceryl ether cinnamic acetal and 0.85 g of menthol were stirred and mixed for 10 min to obtain a composite cooling agent composition;
[0118] S4. Immobilization: Dissolve 0.4 g of the composite cooling agent composition in 20 mL of ethanol, add 1 g of mesoporous hollow silica nanospheres, evaporate the solvent, and prepare composite nanospheres, which are cooling agents.
[0119] Test Example 2 Release Kinetics Study
[0120] The cooling agent samples (weight about 10 g, initial weight m 0 ) were placed in a blast oven at 30°C and 80°C for constant temperature heating (air flow rate 500 cm 3 / min), and at regular intervals, use a precision electronic balance to weigh the mass m of the sample. 1 , record the change in the sample mass, and when the sample is heated to a constant mass, stop heating and measure the weight at this time as m 2 , calculate the release rate (%).
[0121] Release rate (%) = (m 0 -m1) / (m 0 -m 2 )×100%
[0122] The results are shown in Tables 2 and 3.
[0123] Table 2 Changes in release rate under 30℃ air purge
[0124] Group 200min 400min 800min 1600min Example 1 45.6 62.2 72.2 >99.9 Example 2 46.2 62.9 73.9 >99.9 Example 3 46.9 63.1 74.5 >99.9 Comparative Example 1 42.2 60.9 69.8 >99.9 Comparative Example 2 43.9 61.2 71.9 >99.9 Comparative Example 3 44.1 61.5 71.3 >99.9 Comparative Example 4 38.3 55.2 65.1 91.1 Comparative Example 5 44.9 61.1 72.0 >99.9 Comparative Example 6 45.1 61.9 71.8 >99.9 Comparative Example 7 66.9 >99.9 >99.9 >99.9
[0125] It can be seen from the above table that the cooling agents prepared in Examples 1-3 of the present invention have a sustained release effect.
[0126] Table 3 Changes in release rate under 80℃ air purge
[0127] Group 20min 40min 80min 120min Example 1 30.9 56.7 97.8 >99.9 Example 2 31.1 57.2 98.2 >99.9 Example 3 31.8 57.6 98.7 >99.9 Comparative Example 1 28.9 54.2 95.2 >99.9 Comparative Example 2 29.7 55.8 96.6 >99.9 Comparative Example 3 29.1 55.3 96.1 >99.9 Comparative Example 4 24.8 49.5 90.2 97.8 Comparative Example 5 30.2 55.8 96.6 >99.9 Comparative Example 6 29.7 56.1 96.9 >99.9 Comparative Example 7 55.8 98.9 >99.9 >99.9
[0128] It can be seen from the above table that the release rate of the cooling agent prepared in Examples 1-3 of the present invention is significantly accelerated under high temperature conditions.
[0129] Test Example 3
[0130] Take several portions of 10g of unflavored cigarette shreds, accurately weigh 0.10% of the weight of the cooling agent prepared in Examples 1-3 and Comparative Examples 1-7, and use menthol as a control sample, add them to 2mL of 95% ethanol, and spray them evenly on the shredded tobacco with a laryngeal nozzle. The shredded tobacco samples are placed in a constant temperature and humidity chamber at a temperature of (25±1)℃ and a relative humidity of (65±2)% for 24 hours to balance the moisture, and then put into a constant temperature and humidity chamber after being manually rolled, and balanced for another 24 hours under the same conditions, and then evaluated by professionals. The results are shown in Table 4.
[0131] Table 4
[0132]
[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a cooling agent, characterized in that: The following steps are involved: S1. Preparation of mesoporous hollow silica nanospheres: dissolving alkyl orthosilicate and an emulsifier in dichloromethane to obtain an organic phase; dissolving a porogen in water to obtain an aqueous phase; dropping the aqueous phase into the organic phase, emulsifying, adjusting the pH value of the solution, stirring the reaction, centrifuging, washing, drying, and calcining to obtain mesoporous hollow silica nanospheres; S2. Preparation of Menthyl Glyceryl Ether Cinnamaldehyde: Menthyl Glyceryl Ether and Cinnamaldehyde are reacted in the presence of a catalyst to obtain Menthyl Glyceryl Ether Cinnamaldehyde, the structural formula of which is shown in Formula I: S3. Preparation of a composite cooling agent composition: The mint glyceryl ether cinnamic acetal and menthol were uniformly mixed to obtain a composite cooling agent composition; S4. Immobilization: dissolving the composite cooling agent composition in ethanol, adding mesoporous hollow silica nanospheres, and evaporating the solvent to obtain composite nanospheres; S5. Coating: adding the composite nanospheres into water, adding tannic acid and a catalyst, heating and stirring to react, centrifuging, washing, and drying to obtain a cooling agent.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the alkyl orthosilicate, emulsifier and porogen in step S1 is 12-15:0.5-1:1-2, the emulsifier is selected from at least one of Span-20, Span-40, Span-60, Span-80 and Span-85, the porogen is hexadecyltrimethylammonium chloride or hexadecyltrimethylammonium bromide, the pH value of the adjusted solution is 9-10, the stirring reaction time is 10-12h, the calcination temperature is 450-550°C, and the time is 1-3h.
3. The preparation method according to claim 1, characterized in that: In step S2, the molar ratio of menthol ether to cinnamaldehyde is 1-1.1:1, the amount of the catalyst added is 0.5-1wt% of the total mass of the system, the reaction temperature is 70-80°C, the reaction time is 4-6h, and the preparation method of the catalyst is as follows: T1. Preparation of mesoporous silica microspheres: dissolving alkyl orthosilicate and porogen in ethanol, adding ammonia solution to adjust the pH value of the solution, stirring the reaction, centrifuging, washing, drying, and calcining to obtain mesoporous silica microspheres; T2. Preparation of polyvinyl pyrrolidone modified with acidic ionic liquid: adding polyvinyl pyrrolidone to toluene, adding 1,3-propane sultone and 1,4-butane sultone, heating and stirring to react, filtering, washing, drying, adding to ethyl acetate, adding tannic acid and a catalyst, stirring to react, filtering, washing, drying, and obtaining polyvinyl pyrrolidone modified with acidic ionic liquid; T3. Immobilization: Add polyvinyl pyrrolidone modified with acidic ionic liquid into water, add mesoporous silica microspheres, evaporate the solvent at room temperature, and prepare composite microspheres; T4. Preparation of catalyst: dissolve diethylaluminum chloride in n-hexane, add composite microspheres, stir to react, centrifuge, wash, and dry to obtain a catalyst.
4. The preparation method according to claim 3, characterized in that: In step T1, the alkyl orthosilicate is methyl orthosilicate or ethyl orthosilicate, the mass ratio of the alkyl orthosilicate and the porogen is 17-22:1-2, the porogen is hexadecyltrimethylammonium chloride or hexadecyltrimethylammonium bromide, the pH value of the adjusted solution is 8.5-9.5, the stirring reaction time is 7-10h, the calcination temperature is 450-550°C, and the time is 1-3h; in step T2, the mass ratio of polyvinyl pyrrolidone, 1,3-propane sultone, 1,4-butane sultone, tannic acid and catalyst is 10:3-4:2-3:7-10:0.5-1, the catalyst has a pH of 8.5-9.5 Tris-HCl solution, the heating and stirring reaction temperature is 75-85°C, the time is 20-24h, and the stirring reaction time is 3-5h.
5. The preparation method according to claim 3, characterized in that: The mass ratio of the acidic ionic liquid-modified polyvinyl pyrrolidone to the mesoporous silica microspheres in step T3 is 3-5:10; the mass ratio of diethylaluminum chloride to the composite microspheres in step T4 is 2-3:10, and the stirring reaction time is 0.5-1.5h.
6. The preparation method according to claim 1, characterized in that: The mass ratio of the menthyl ether cinnamic acetal to menthol in step S3 is 4-6:7-10.
7. The preparation method according to claim 1, characterized in that: The mass ratio of the composite cooling agent composition and the mesoporous hollow silica nanospheres in step S4 is 3-5:
10.
8. The preparation method according to claim 1, characterized in that: The mass ratio of the composite nanospheres, tannic acid and catalyst in step S5 is 10:7-12:0.5-1, the temperature of the heating and stirring reaction is 35-45°C, the time is 2-4h, and the pH of the catalyst is Tris-HCl solution of 8.5-9.
5.
9. A cooling agent prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the cooling agent according to claim 9 in cigarettes.