Preparation method and application of sustained and controlled release hydroxypropyl methylcellulose

Through the supercritical carbon dioxide extraction process, the problems of complex process and high energy consumption in the preparation of hydroxypropyl methylcellulose are solved, and high pressure and high flowability products are achieved, the process is simplified and wastewater is reduced, and the production of wastewater is improved. Quality and production efficiency of the preparation.

CN118930663APending Publication Date: 2024-11-12JIANGSU XIDIAN PHARM EXCIPIENTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411235546.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the preparation process of hydroxypropyl methylcellulose is complex, has high energy consumption, and has a large amount of wastewater, and is difficult to meet the requirements of high compressibility and high flowability, which affects the quality and production efficiency of the slow-release formulation.

Method used

The supercritical carbon dioxide extraction process is adopted to carry out etherification reaction through alkalizing and etherified cotton pulp or wood pulp, and one-step purification is used to remove by-products and impurities, thereby improving the compressibility of hydroxypropyl methylcellulose and Liquidity.

Benefits of technology

The preparation of high-pressure and high-flowability hydroxypropyl methylcellulose is achieved, the process flow is simplified, energy consumption and wastewater production is reduced, the quality and production efficiency of the preparation is improved, and it is environmentally friendly and green.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930663A_ABST
    Figure CN118930663A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sustained and controlled release preparations, and particularly discloses a preparation method and application of sustained and controlled release hydroxypropyl methylcellulose, and the preparation method comprises the following steps: adding cotton pulp or wood pulp, a dispersing agent and a sodium hydroxide aqueous solution into a reaction kettle, sealing the reaction kettle, carrying out nitrogen vacuum replacement, and carrying out heat preservation alkalization for 2 hours; after alkalization is completed, epoxypropane and chloromethane are sequentially introduced, etherification reaction is carried out, and after etherification is completed, emptying is carried out, and redundant epoxypropane and chloromethane are recovered; the method comprises the following steps: directly pressing a mixed solution of a hydroxypropyl methylcellulose crude product, a byproduct and the like into an extraction tank, circularly extracting the mixed solution by using supercritical carbon dioxide fluid, and further crushing and screening to obtain the high sustained and controlled release hydroxypropyl methylcellulose. A large amount of waste water is not generated, the method is efficient, energy-saving, green and environment-friendly, meanwhile, the product can be bulked, and higher compressibility is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sustained-release preparations, and in particular relates to a preparation method and application of sustained-release hypromellose. Background Art

[0002] Sustained-release preparations refer to preparations that use coating technology or skeleton materials to reduce the release rate of drugs and reduce the peak and valley phenomenon of drug concentration, thereby achieving better therapeutic effects. Its advantages include: reducing the frequency of administration, reducing the total dosage of the drug, reducing toxic side effects, and reducing irritation to the gastrointestinal tract. Among oral sustained-release tablets, hydrophilic gel skeleton tablets are widely used due to their small drug release variability, high safety, simple process, low cost, and mature process. The most commonly used hydrophilic gel skeleton material is hydroxypropyl methylcellulose.

[0003] With the continuous development of formulation technology, in order to adapt to the increasingly complex dosage form requirements, pharmaceutical excipients are also constantly meeting the needs of formulations.

[0004] Hydroxypropyl methylcellulose can be used as a multifunctional excipient in pharmaceuticals for sustained-release preparations, plant capsules, tablet coating films, thickeners / suspending agents, tablet adhesives, tablet disintegrants, etc. Its material properties vary in different functional requirements. When used as a sustained-release functional excipient, in addition to meeting the physical and chemical indicators of the pharmacopoeia, its compressibility and fluidity are also key material properties, which are particularly prominent in advanced direct compression preparation processes. The products on the market that meet the compressibility requirements of sustained-release preparations mainly include Dow Japan Shin-Etsu wait.

[0005] Patent CN107915781 discloses a method for synthesizing hypromellose used in sustained-release preparations, which describes mixing sodium hydroxide and wood pulp or cotton pulp to prepare alkaline cellulose, then adding methyl chloride and propylene oxide to react to obtain hypromellose, and then washing, granulating, drying, secondary granulating, synchronous drying and crushing to obtain high-flowability and high-compressibility sustained-release hypromellose. The hypromellose obtained by this method has a complex process, high energy consumption, and a large amount of wastewater.

[0006] Patent CN103880966B discloses a method for preparing a controlled-release hydroxypropyl methylcellulose, which comprises adding a solvent containing a phase transfer catalyst, fatty alcohol polyoxyethylene ether, to cellulose pulp, then adding sodium hydroxide, propylene oxide, and methyl chloride, and then recovering the solvent, washing, separating, and drying to obtain a product with excellent controlled-release performance. This method adds fatty alcohol polyoxyethylene ether, which increases the difficulty of impurity removal for pharmaceutical excipients, and consumes a large amount of hot water, resulting in increased energy consumption. At the same time, its compressibility and fluidity are not mentioned, which increases the requirements for the preparation process of the sustained-release material and increases the cost of the preparation equipment.

[0007] Methods for using hypromellose in sustained-release preparations include, but are not limited to, dry premixing of the drug, hypromellose and other excipients followed by dry direct tableting; wet or dry granulation, drying, and crushing of the drug and other excipients followed by adding hypromellose and mixing for tableting.

[0008] In the common tablet production process, if HPMC does not have high compressibility or high fluidity, the resulting tablets will not be hard enough or uniform enough, which can easily cause unpredictable tablet breakage and affect the sustained-release effect. To deal with HPMC with low compressibility and fluidity, the formulation process needs to use more complex and higher-strength production equipment such as premixers and tablet presses, which is usually unstable and uneconomical.

[0009] At the same time, in the existing process, the crude hydroxypropyl methylcellulose and by-products synthesized from cotton pulp / wood pulp through alkalization and etherification need to go through the steps of neutralization, desolventization, hot water desalination, dehydration, crushing and screening in sequence. The process is complicated, energy consumption is high, and a large amount of wastewater and organic solvent mixture is generated, which will cause certain pollution to the environment.

[0010] The hypromellose produced by the invention provides a method for preparing sustained-release hypromellose with high compressibility and high fluidity in order to make up for the defects of the prior art products. Summary of the invention

[0011] The object of the present invention is to provide a preparation method and application of sustained-release hypromellose to solve the problems raised in the above-mentioned background technology.

[0012] To achieve the above object, the present invention provides the following technical solutions:

[0013] A method for preparing sustained-release hypromellose comprises the following steps:

[0014] Step 1: In a reaction kettle, add 1 part of a base material, which is cotton pulp or wood pulp, 5-15 parts of a dispersant, and 1-3 parts of a sodium hydroxide aqueous solution, seal the reaction kettle, replace the nitrogen vacuum for 3 times, and then keep the temperature at 20-50° C. for alkalization for 2 hours;

[0015] Step 2: After the alkalization is completed, the vacuum is reduced to less than -0.096 MPa, and propylene oxide and methyl chloride are introduced in sequence, and the etherification reaction is carried out at 40-60° C. and 70-90° C. for 2-4 hours, respectively. The pressure of the reactor during the etherification process is controlled at 0.5-1.0 MPa. After the etherification is completed, the excess propylene oxide and methyl chloride are emptied and recovered;

[0016] Step 3, directly press the crude hydroxypropyl methylcellulose and the mixed solution of the by-product into the extraction tank, the closed system, the cylinder carbon dioxide enters the system through the pressure reducing valve and the water removal device, and then enters the buffer tank through the condenser and the pressure pump, and flows into the extraction tank after reaching the supercritical pressure extraction pressure, during which the temperature is raised to the supercritical temperature extraction temperature by the pipeline heater to obtain the supercritical carbon dioxide fluid, when the supercritical carbon dioxide fluid flow passes through the extraction tank at the initial stage, the solution in the by-product together with the soluble substances will be filtered out of the extraction tank, and the crude hydroxypropyl methylcellulose will be intercepted by the filter screen set at the outlet of the extraction tank, when the supercritical carbon dioxide circulates through the extraction tank for many times, the supercritical carbon dioxide will use its high solubility to repeatedly extract the by-products and impurities in the crude hydroxypropyl methylcellulose, without affecting the hydroxypropyl methylcellulose itself;

[0017] Step 4: After supercritical carbon dioxide extraction, the remaining material in the extraction tank is pure hypromellose, which is further crushed and screened to obtain high-compressibility, high-flowability sustained-release hypromellose.

[0018] Preferably, in step 1, the dispersant is one or more of C5-C8 alkanes, dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, propylene glycol dimethyl ether, dipropylene glycol dimethyl ether, toluene, xylene, and C1-C4 alcohols.

[0019] Preferably, in step three, the extraction pressure is 8MPa-20MPa, the extraction temperature is 40°C-90°C, and the cycle extraction time is 0.5h-12h.

[0020] Preferably, in step three, the by-product mixed solution obtained by extraction includes one or more of the dispersants mentioned in step one, as well as water, by-product sodium salt, by-product propylene glycol and its derivatives, which will be further separated and collected in a separator for reuse.

[0021] The hydroxypropyl methylcellulose prepared by the present invention can be specifically used as a hydrophilic gel skeleton material.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The invention provides a method for preparing a highly compressible and highly fluid sustained-release hydroxypropyl methylcellulose. After the cotton pulp / wood pulp is synthesized through alkalization and etherification, a one-step purification process is innovatively performed using supercritical carbon dioxide. This process completes the processes of neutralization, desolventization, dehydration, removal of by-product sodium salt, removal of by-product propylene glycol and its derivatives, and fluffing products in one set of equipment. It does not require multiple material transfers, does not require a dedicated solvent recovery device, does not generate a large amount of wastewater, is highly efficient and energy-saving, and is green and environmentally friendly.

[0024] 2. The present invention efficiently utilizes by-product propylene glycol and its derivatives as supercritical carbon dioxide entrainers, forms a microemulsion in a supercritical fluid under the joint action of hydrophilic groups and lipophilic groups, and efficiently separates organic solvents, water and other substances, and desolventization and dehydration are completed simultaneously.

[0025] 3. The present invention uses excess supercritical carbon dioxide, part of which neutralizes excess sodium hydroxide in the raw material to generate sodium carbonate or sodium bicarbonate, most of the sodium carbonate, sodium bicarbonate and other sodium salts are taken out of the system by the microemulsion in the supercritical fluid, and a small amount of sodium carbonate and sodium bicarbonate are stored in the system as chemical microfoaming agents, and cooperate with the supercritical carbon dioxide as a physical microfoaming agent to make the product fluffy and provide higher compressibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the process of the present invention;

[0027] Figure 2 It is a relationship diagram between compaction strength and tensile strength of granular materials in the present invention;

[0028] Figure 3 It is a comparison curve of the sustained-release effect of the reference preparation and the example in the sustained-release preparation of the present invention. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Embodiment 1:

[0031] See also Figure 1 - Figure 3 As shown, the production process of preparing sustained-release hypromellose by supercritical carbon dioxide process comprises the following steps in sequence:

[0032] Step 1: In a reaction kettle, add 1 part of wood pulp, 5 parts of dimethyl ether, and 1 part of sodium hydroxide aqueous solution, seal the reaction kettle, replace the nitrogen vacuum for 3 times, and then keep the temperature at 20°C for alkalization for 2 hours;

[0033] Step 2: After the alkalization is completed, the vacuum is reduced to less than -0.096 MPa, and propylene oxide and methyl chloride are introduced in sequence, and the etherification reaction is carried out at 50° C. and 80° C. for 2 hours, respectively. The pressure of the reactor during the etherification process is controlled at 1.0 MPa. After the etherification is completed, the excess propylene oxide and methyl chloride are emptied and recovered;

[0034] Step 3: directly press the crude hydroxypropyl methylcellulose and the by-product mixed solution into the extraction tank, and after the system is closed, the supercritical carbon dioxide fluid that has been condensed, pressurized and heated is circulated to extract the mixed solution, the extraction pressure is 8MPa, the extraction temperature is 40°C, and the cyclic extraction time is 10h;

[0035] Step 4: After supercritical carbon dioxide extraction, the remaining material in the extraction tank is pure hydroxypropyl methylcellulose, which is crushed by a centrifugal grinder and sieved to obtain high-compressibility and high-flowability sustained-release hydroxypropyl methylcellulose.

[0036] Embodiment 2:

[0037] See also Figure 1 - Figure 3 As shown, the production process of preparing sustained-release hypromellose by supercritical carbon dioxide process comprises the following steps in sequence:

[0038] Step 1: Add 1 part of cotton pulp, 10 parts of toluene / isopropanol mixture, and 2 parts of sodium hydroxide aqueous solution into a reaction kettle, seal the reaction kettle, replace the nitrogen vacuum for 3 times, and then keep the temperature at 40°C for 2 hours;

[0039] Step 2: After the alkalization is completed, the vacuum is reduced to less than -0.096 MPa, and propylene oxide and methyl chloride are introduced in sequence, and the etherification reaction is carried out at 40° C. and 90° C. for 2 hours, respectively. The pressure of the reactor during the etherification process is controlled at 1.0 MPa. After the etherification is completed, the excess propylene oxide and methyl chloride are emptied and recovered;

[0040] Step 3: directly press the crude hydroxypropyl methylcellulose and the mixed solution of the by-product into the extraction tank, and after the system is closed, the supercritical carbon dioxide fluid that has been condensed, pressurized and heated is circulated to extract the mixed solution, the extraction pressure is 10MPa, the extraction temperature is 50°C, and the cyclic extraction time is 6h;

[0041] Step 4: After supercritical carbon dioxide extraction, the remaining material in the extraction tank is pure hypromellose, which is crushed by a turbine grinder and sieved to obtain high-compressibility and high-flowability sustained-release hypromellose.

[0042] Wherein in step one described in the preparation process, the dispersant is one or more of C5-C8 alkane, dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, propylene glycol dimethyl ether, dipropylene glycol dimethyl ether, toluene, xylene, C1-C4 alcohol, and in the present invention, the extraction pressure in step three is 8MPa-20MPa, the extraction temperature is 40°C-90°C, and the cycle extraction time is 0.5h-12h. In the present invention, in step four, one or more of the dispersants mentioned in step one, as well as water, by-product sodium salt, by-product propylene glycol and its derivatives are extracted, and further separated and collected in a separator for reuse. In step four, the crushing can be performed by selecting equipment such as a mechanical crusher, a ball mill, a centrifugal crusher, an impact crusher, a turbine crusher, a cutting crusher, etc., until the particle size meets the requirements.

[0043] Comparative Example 1:

[0044] The existing process for preparing sustained-release hypromellose comprises the following steps in sequence:

[0045] Step 1: In a reaction kettle, add 1 part of wood pulp, 5 parts of dimethyl ether, and 1 part of sodium hydroxide aqueous solution, seal the reaction kettle, replace the nitrogen vacuum for 3 times, and then keep the temperature at 20°C for alkalization for 2 hours;

[0046] Step 2: After the alkalization is completed, the vacuum is reduced to less than -0.096 MPa, and propylene oxide and methyl chloride are introduced in sequence, and the etherification reaction is carried out at 50° C. and 80° C. for 2 hours, respectively. The pressure of the reactor during the etherification process is controlled at 1.0 MPa. After the etherification is completed, the excess propylene oxide and methyl chloride are emptied and recovered;

[0047] Step 3, the crude hydroxypropyl methylcellulose and the mixed solution of the by-product are neutralized with acetic acid or hydrochloric acid in the etherification kettle, transferred to the desolventizing kettle for high-temperature filtration, desolventizing and dehydration, and then transferred to the washing kettle to add 10 parts of freshly boiled hot water to repeatedly wash the crude hydroxypropyl methylcellulose to remove the by-product sodium salt and by-product propylene glycol and its derivatives. The entire product transfer process requires high-temperature heating;

[0048] Step 4: After multiple high-temperature and large-volume hot water washings, the wet product of hypromellose is simultaneously dried and crushed by an impact mill, and then sieved to obtain hypromellose powder.

[0049] Table 1 Physical parameters of product powder and evaluation results

[0050]

[0051]

[0052] Depend on Figure 2 It can be seen that the product prepared by Example 1 of the present invention has the highest tensile strength. Figure 3It can be seen that the sustained-release effect comparison of the product prepared in the embodiment of the present invention is consistent with that of the reference preparation.

[0053] The product prepared in the present invention has an average particle size of 90-120 μm, a bulk density of 0.28-0.32 g / ml, an angle of repose of less than 40°, and good fluidity. At the same time, the product prepared in the present invention is subjected to a compaction pressure of 30-40 MPa to produce a hard sheet with a tensile strength of not less than 0.17 MPa, and the product has good compressibility.

[0054] Meanwhile, the product prepared in the present invention has a methoxyl substitution degree of 1.0-2.0%, a hydroxypropoxyl substitution degree of 0.2-0.5%, and a viscosity of 50-200000 cps, which is measured by a rotational viscometer for a 2 wt % aqueous solution thereof. The product can be used as a water-soluble gel skeleton material for sustained and controlled release.

[0055] Figure 2 The product is compacted by a tablet punch, and the tensile strength is directly measured by a tablet hardness tester. Imported 1, 2, and domestic 1, 2 all use 100,000 viscosity products of hydroxypropyl methylcellulose 2208 that conform to the Chinese Pharmacopoeia.

[0056] Public data show that the raw materials used in the reference preparation contain hydroxypropyl methylcellulose 2208 type 100,000 viscosity product, and then the metformin hydrochloride sustained-release tablets are prepared using the imported 1 and the product prepared in the present invention according to the public prescription.

[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing sustained-release hypromellose, characterized in that: The following steps are involved: Step 1: In a reaction kettle, add 1 part of a base material, which is cotton pulp or wood pulp, 5-15 parts of a dispersant, and 1-3 parts of a sodium hydroxide aqueous solution, seal the reaction kettle, replace the nitrogen vacuum for 3 times, and then keep the temperature at 20-50° C. for alkalization for 2 hours; Step 2: After the alkalization is completed, the vacuum is reduced to less than -0.096 MPa, and propylene oxide and methyl chloride are introduced in sequence, and the etherification reaction is carried out at 40-60° C. and 70-90° C. for 2-4 hours, respectively. The pressure of the reactor during the etherification process is controlled at 0.5-1.0 MPa. After the etherification is completed, the excess propylene oxide and methyl chloride are emptied and recovered; Step 3, directly press the crude hydroxypropyl methylcellulose and the mixed solution of the by-product into the extraction tank, the closed system, the cylinder carbon dioxide enters the system through the pressure reducing valve and the water removal device, and then enters the buffer tank through the condenser and the pressure pump, and flows into the extraction tank after reaching the supercritical pressure extraction pressure, during which the temperature is raised to the supercritical temperature extraction temperature by the pipeline heater to obtain the supercritical carbon dioxide fluid, when the supercritical carbon dioxide fluid flow passes through the extraction tank at the initial stage, the solution in the by-product together with the soluble substances will be filtered out of the extraction tank, and the crude hydroxypropyl methylcellulose will be intercepted by the filter screen set at the outlet of the extraction tank, when the supercritical carbon dioxide circulates through the extraction tank for many times, the supercritical carbon dioxide will use its high solubility to repeatedly extract the by-products and impurities in the crude hydroxypropyl methylcellulose, without affecting the hydroxypropyl methylcellulose itself; Step 4: After supercritical carbon dioxide extraction, the remaining material in the extraction tank is pure hypromellose, which is further crushed and screened to obtain high-compressibility, high-flowability sustained-release hypromellose.

2. The method for preparing a sustained-release hypromellose according to claim 1, characterized in that: In the step 1, the dispersant is one or more of C5-C8 alkanes, dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, propylene glycol dimethyl ether, dipropylene glycol dimethyl ether, toluene, xylene, and C1-C4 alcohols.

3. The method for preparing a sustained-release hypromellose according to claim 1, characterized in that: In the step three, the extraction pressure is 8MPa-20MPa, the extraction temperature is 40°C-90°C, and the cycle extraction time is 0.5h-12h.

4. The method for preparing a sustained-release hypromellose according to claim 1, characterized in that: In step three, the by-product mixed solution obtained by extraction includes one or more of the dispersants mentioned in step one, as well as water, by-product sodium salt, by-product propylene glycol and its derivatives, which will be further separated and collected in a separator for reuse.

5. The method for preparing sustained-release hypromellose according to claim 1, characterized in that: In the step 4, the pulverization can be performed by using one of a mechanical pulverizer, a ball mill, a centrifugal pulverizer, an impact pulverizer, a turbine pulverizer, and a cutting pulverizer.

6. Use of the hypromellose prepared by the method for preparing sustained-release hypromellose according to claim 1 as a hydrophilic gel skeleton material in a preparation.