Method for preparing amidoxime material by using microfluidics and application of amidoxime material

Amidoxime polyacrylonitrile resin material prepared through microfluidic control technology solves the problems of the existing bauxite gallium extracting adsorbent process and small adsorption capacity, realizes efficient gallium ion recovery, and provides higher adsorption capacity and stability.

CN118930688APending Publication Date: 2024-11-12CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410989215.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing bauxite gallium extract adsorbents such as chelating resins have complex preparation processes and many organic reagents are used, resulting in the production of organic wastewater, and the adsorption capacity is small and easy to break, making it impossible to effectively recover gallium ions.

Method used

The amidoxime polyacrylonitrile resin material is prepared by microfluidic control technology. By mixing polyacrylonitrile powder, pore-generating agent and organic solvent, the polyacrylonitrile solution is controlled to be added to the solvent, and then reacted with water and hydroxylamine to adjust the pH value. Form a porous material to increase the adsorption capacity of gallium ions.

Benefits of technology

The prepared amidoxime polyacrylonitrile resin material has high adsorption capacity, high group grafting rate and large surface area. It is suitable for efficient recovery of gallium ions in vanadium sludge, and solves the small adsorption capacity of existing adsorbents and Prone to broken problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958398460000051
    Figure BDA0004958398460000051
  • Figure HDA0004958398470000011
    Figure HDA0004958398470000011
  • Figure HDA0004958398470000012
    Figure HDA0004958398470000012
Patent Text Reader

Abstract

The invention provides a method for preparing an amidoxime polyacrylonitrile resin material by microfluidics and application of the amidoxime polyacrylonitrile resin material, and the method comprises the following steps: 1) mixing polyacrylonitrile powder, a pore-foaming agent and an organic solvent to obtain a polyacrylonitrile solution; 2) absorbing the polyacrylonitrile solution, and controlling the polyacrylonitrile solution to be added into a solvent in a microfluidic mode to obtain polyacrylonitrile resin with uniform size; 3) mixing and dissolving the polyacrylonitrile resin, water and a hydroxylamine reagent to obtain a resin modified liquid; 4) adjusting the pH value of the resin modified liquid, reacting, and filtering to obtain a porous material; and 5) dispersing, filtering and drying the porous material to obtain the amidoxime material. The material prepared by the method has high gallium adsorption capacity. The grafting rate of an amidoxime group of the amidoxime polyacrylonitrile resin material is 68-97%; bET is from 11.7 to 13.6 m < 2 > / g; the average particle size is 1.9 to 2.4 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and in particular relates to a method for preparing amidoxime material by using microfluidics and application thereof. Background Art

[0002] With the booming development of the semiconductor field, the demand for gallium is also increasing. The gallium content in the vanadium sludge obtained by smelting vanadium-titanium magnetite is relatively high, reaching the industrial mining grade, and the stockpile is large. Therefore, it can be regarded as one of the alternative sources of gallium. The method for recovering gallium from smelting products related to vanadium-titanium magnetite is mainly to use solvent extraction. CN115369244A is a method for selectively extracting gallium from alkaline leaching solution of vanadium tailings based on microemulsion. The limitations of microemulsion extraction are relatively large, and the synthesis process is relatively difficult. Therefore, the adsorption method is still one of the preferred methods for recovering gallium from the solution.

[0003] At present, the main raw material for gallium extraction is the Bayer solution of bauxite, and the existing adsorbents for gallium extraction from bauxite mostly use chelating resins to adsorb gallium in the Bayer mother liquor. However, the preparation method of chelating resins has the problem of long synthesis process and more organic reagents used, which in turn produces more organic wastewater. Patent CN1454706 A A chelating resin for gallium adsorption and preparation method and patent CN101875004A A chelating resin for gallium adsorption, its preparation method and its application are both for alkaline solutions of bauxite, but the existing commercial resins have problems such as small adsorption capacity and easy breakage during use due to their low functional group grafting rate and small specific surface area. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a method for preparing amidoxime polyacrylonitrile resin material by using microfluidics and its application. The amidoxime polyacrylonitrile resin material prepared by the method has a high adsorption capacity for gallium.

[0005] The present invention provides a method for preparing amidoxime polyacrylonitrile resin material by using microfluidics, comprising the following steps:

[0006] 1) mixing polyacrylonitrile powder, a porogen and an organic solvent to obtain a polyacrylonitrile solution;

[0007] 2) absorbing the polyacrylonitrile solution, and adding the polyacrylonitrile solution to the solvent by microfluidics to obtain polyacrylonitrile resin with uniform size;

[0008] 3) mixing the polyacrylonitrile resin, water and hydroxylamine reagent, dissolving them, and obtaining a resin modified liquid;

[0009] 4) adjusting the pH value of the resin modified liquid, and reacting to obtain a porous material;

[0010] 5) dispersing, filtering and drying the porous material to obtain amidoxime polyacrylonitrile resin material.

[0011] Preferably, the flow rate of the microfluidic method in step 2) is 5 to 20 mL / min.

[0012] Preferably, the molecular weight of the polyacrylonitrile powder in step 1) is 150,000 to 1,000,000;

[0013] The porogen is one or more of polyvinyl pyrrolidone, sucrose, sodium chloride and polyethylene glycol;

[0014] The organic solvent is selected from one or more of N'N-dimethylformamide, N'N-dimethylacetamide, dimethyl sulfoxide, isopropyl acetate and tetrahydrofuran.

[0015] Preferably, the reagent in step 2) is pure water, alcohol or an alcohol-water mixture.

[0016] Preferably, the mass ratio of the liquid volume to the solid material in the resin modification liquid in step 3) is (5-20) mL:1 g;

[0017] The molar ratio of the hydroxylamine to the polyacrylonitrile is 1:1 to 4:1.

[0018] Preferably, in step 4), solid base is used to adjust the pH value;

[0019] The solid alkali is selected from one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, potassium bicarbonate, sodium bicarbonate and ammonium bicarbonate.

[0020] Preferably, in step 4), the reaction temperature is 50-90° C. and the reaction time is 2-6 hours.

[0021] Preferably, in step 5), the porous material is dispersed using anhydrous ethanol, and the dispersion time is 10 to 60 minutes.

[0022] The drying temperature is -40℃~0℃, and the drying time is 6~12h.

[0023] The present invention provides an application of an amidoxime polyacrylonitrile resin material prepared by the method described in the above technical scheme in recovering gallium ions from a vanadium-extracting sludge acid leaching solution.

[0024] The present invention provides a method for preparing amidoxime polyacrylonitrile resin material by microfluidics, comprising the following steps: 1) mixing polyacrylonitrile powder, porogen and organic solvent to obtain polyacrylonitrile solution; 2) absorbing the polyacrylonitrile solution, and controlling the polyacrylonitrile solution to be added to the solvent by microfluidics to obtain polyacrylonitrile resin of uniform size; 3) mixing the polyacrylonitrile resin with water and hydroxylamine reagent, dissolving to obtain resin modified liquid; 4) adjusting the pH value of the resin modified liquid, reacting, filtering to obtain a porous material; 5) dispersing, filtering and drying the porous material to obtain an amidoxime material. The amidoxime polyacrylonitrile resin material prepared by the method provided by the present invention has a high adsorption capacity for gallium. The amidoxime polyacrylonitrile resin material prepared by the method provided by the present invention has a grafting rate of amidoxime groups of 68-97%; the BET of the amidoxime polyacrylonitrile resin material is 11.7-13.6 m 2 / g; the average particle size of the amidoxime polyacrylonitrile resin material is 1.9 to 2.4 mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of the process of preparing polyacrylonitrile resin of uniform size by microfluidics in Example 1 of the present invention;

[0026] Figure 2 is a scanning electron microscope image of the polyacrylonitrile resin and the amidoxime material in Example 1 of the present invention;

[0027] Figure 3 This is a schematic diagram of a finished product modified with fiber amidoxime according to patent CN106824138A;

[0028] Figure 4 is a trend diagram of the change of gallium adsorption content of AOPAN over time in Example 2 of the present invention;

[0029] Figure 5 This is a scanning electron microscope image of the amidoxime material after adsorption of gallium in Example 3 of the present invention;

[0030] Figure 6 Infrared spectra of polyacrylonitrile powder, polyvinyl pyrrolidone, polyacrylonitrile resin, and amidoxime polyacrylonitrile resin in Example 5 of the present invention;

[0031] Figure 7 This is the infrared spectrum of AOPAN before and after adsorption of gallium in Example 5 of the present invention. DETAILED DESCRIPTION

[0032] The present invention provides a method for preparing amidoxime polyacrylonitrile resin material by using microfluidics, comprising the following steps:

[0033] 1) mixing polyacrylonitrile powder, a porogen and an organic solvent to obtain a polyacrylonitrile solution;

[0034] 2) absorbing the polyacrylonitrile solution, and adding the polyacrylonitrile solution to the solvent by microfluidics to obtain polyacrylonitrile resin with uniform size;

[0035] 3) mixing the polyacrylonitrile resin, water and hydroxylamine reagent, dissolving them, and obtaining a resin modified liquid;

[0036] 4) adjusting the pH value of the resin modified liquid, reacting, filtering, and obtaining a porous material;

[0037] 5) dispersing, filtering and drying the porous material to obtain amidoxime polyacrylonitrile resin material.

[0038] The present invention mixes polyacrylonitrile powder, porogen and organic solvent to obtain polyacrylonitrile solution. The present invention preferably places polyacrylonitrile powder and porogen in a three-necked beaker, then mixes with organic solvent, stirs, mixes evenly, and the solution is transparent and light yellow.

[0039] The molecular weight of the polyacrylonitrile powder in the present invention is 150,000 to 1,000,000; specifically, the molecular weight is 150,000, 250,000, 500,000 or 1,000,000. The porogen is one or more of polyvinyl pyrrolidone (PVP), sucrose, sodium chloride and polyethylene glycol; the organic solvent is one or more of N'N-dimethylformamide, N'N-dimethylacetamide, dimethyl sulfoxide, isopropyl acetate and tetrahydrofuran. The organic solvent can dissolve the polyacrylonitrile powder and the porogen.

[0040] In the present invention, the mass of polyacrylonitrile powder, the mass of porogen and the volume ratio of organic solvent are (0.5-2) g: (1-5) g: (10-30) mL.

[0041] After obtaining the polyacrylonitrile solution, the present invention absorbs the polyacrylonitrile solution, and controls the polyacrylonitrile solution to be added into the solvent by microfluidics to obtain polyacrylonitrile resin with uniform size.

[0042] The present invention preferably uses a needle tube to absorb the above-mentioned polyacrylonitrile solution; the needle type of the pipette is 15G to 23G; in a specific embodiment, the needle type used is 20G or 22G. The present invention implements a microfluidic method through a microfluidic pump, and the flow rate used in the microfluidic method is 5 to 20mL / h; in a specific embodiment, the flow rate is 10mL / h. In the present invention, the microfluidic pump is driven at a certain speed to release the polyacrylonitrile solution into a solvent; the solvent is pure water, alcohol, or an alcohol-water mixture.

[0043] The polyacrylonitrile solution is added to the solvent by microfluidics and then preferably allowed to stand for 25 to 40 minutes to remove the porogen. After the standing, the solution is filtered to obtain solid particles of uniform size.

[0044] The present invention mixes the obtained polyacrylonitrile resin with water and a hydroxylamine reagent, dissolves, and obtains a resin modified liquid. The present invention preferably adds solid particles to a three-necked flask, adds water, and then adds a hydroxylamine reagent, stirs evenly, and obtains a solution. The hydroxylamine reagent in the present invention is hydroxylamine hydrochloride. The mass ratio of the volume of the liquid in the resin modified liquid in the step 3) to the solid material is (5 to 20) mL: 1 g; the molar ratio of the hydroxylamine to the polyacrylonitrile is 1: 1 to 4: 1.

[0045] After obtaining the solution, the present invention adjusts the pH value of the resin modified liquid, reacts, and filters to obtain a porous material. The present invention preferably uses a solid base to adjust the pH value, and the solid base is selected from one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, potassium bicarbonate, sodium bicarbonate and ammonium bicarbonate; the pH value is adjusted to 6 to 8, preferably 7. The reaction described in the present invention is a grafting modification reaction; the reaction temperature is 50 to 90°C, and the reaction time is 2 to 6 hours. After the reaction is completed, the reaction solution is filtered and then washed with pure water several times to obtain a porous material.

[0046] After obtaining the porous material, the present invention disperses the porous material, filters, and dries it to obtain amidoxime polyacrylonitrile resin (AOPAN). The agglomeration phenomenon between the porous materials after washing is not weakened, and it is preferably placed in anhydrous ethanol for dispersion treatment; the dispersion time is 10 to 60 minutes, preferably 25 to 35 minutes, and more preferably 28 to 32 minutes. After dispersion, it is filtered and then dried; the drying temperature is -40°C to 0°C, and the time is 6 to 12 hours.

[0047] The amidoxime material prepared by the method provided by the present invention is an amidoxime polyacrylonitrile resin, and the group grafting rate is 68-97%; the BET of the amidoxime material is 11.7-13.6m 2 / g; the average particle size of the amidoxime material is 1.9-2.4 mm. The amidoxime material in the present invention is flat and oval, and belongs to a capsule product.

[0048] The present invention also provides an application of the amidoxime polyacrylonitrile resin material prepared by the method described in the above technical solution in recovering gallium ions from vanadium-extracting sludge acid leaching liquid.

[0049] The present invention uses the following formula to calculate the gallium ion adsorption capacity of the porous material:

[0050]

[0051] Among them, C0 and C e are the initial concentration and equilibrium concentration of the metal in the solution (mg / L), q e is the adsorption capacity (mg / g), V is the total working volume of the solution (mL), and m is the dry weight of the adsorbent (g).

[0052] The adsorption amount of gallium by the amidoxime material provided by the invention is 30-56 mg / g.

[0053] In order to further illustrate the present invention, a method for preparing amidoxime polyacrylonitrile resin material by microfluidics and its application provided by the present invention are described in detail below in combination with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0054] Example 1

[0055] Weigh 1.5g PAN (Da = 150000) powder and 3.5g PVP powder in a 25mL beaker, add 20mL DMF solution (AR grade reagent) in the beaker, and heat and dissolve in a water bath with magnetic stirring until the solution is clear and transparent. Transfer the polyacrylonitrile mixed solution to a 5mL syringe with a 20G needle, and use a microflow pump to uniformly add it to the anhydrous ethanol solution at a speed of 10mL / h. After the reaction is completed, let it stand for 30 minutes to remove the PVP molecules, and filter to obtain polyacrylonitrile resin of uniform size.

[0056] Figure 1 Schematic diagram of the process of preparing polyacrylonitrile resin of uniform size by microfluidic control in Example 1 of the present invention; Figure 1 It can be seen that the polyacrylonitrile resin particles are uniform in size.

[0057] Weigh 1g of polyacrylonitrile resin into a 250ml single-mouth flask, add 1.2g of hydroxylamine hydrochloride into the 250ml single-mouth flask, add 200ml of water to dissolve the hydroxylamine hydrochloride to obtain a resin modified liquid; then add 0.69g of sodium hydroxide into the single-mouth flask, after the sodium hydroxide is completely dissolved, weigh 1g of polyacrylonitrile resin and put it into the flask, transfer the flask to a 60°C water bath, react for 120min at a certain stirring rate, after the reaction is completed, filter with a filter device, and then rinse with pure water for several times. After washing, put the obtained material into anhydrous ethanol for dispersion for 30min, filter after dispersion, and finally put the material into a freeze dryer for drying to obtain amidoxime polyacrylonitrile resin material.

[0058] Figure 2 is a scanning electron microscope image of the polyacrylonitrile resin and the amidoxime material in Example 1 of the present invention; Figure 2 It can be seen that both polyacrylonitrile resin and amidoxime polyacrylonitrile resin are composed of C, H, and O elements and contain rich pore structures. The grafting reaction does not damage the resin pores.

[0059] Figure 3The schematic diagram of the finished product modified with amidoxime according to patent CN106824138A shows that the material shape and the grafting rate of amidoxime groups are inversely proportional, and it is impossible to take both the material shape and the grafting rate of amidoxime into account. However, the amidoxime material prepared in this application can take both the grafting rate of amidoxime and the material morphology into account.

[0060] The amidoxime polyacrylonitrile resin material obtained in Example 1 was used to recover gallium ions from the acid leaching solution of vanadium sludge. The grafting rate of the porous material group was 68%, and the BET was 11.79 m 2 / g, the average particle size is 2.33mm, and the adsorption capacity is 30.12mg / g.

[0061] Example 2

[0062] Weigh 1.5g PAN (Da = 150000) powder and 3.5g PVP powder in a 25mL beaker, add 20mL DMF solution to the beaker, and heat and dissolve in a water bath with magnetic stirring until the solution is clear and transparent. Transfer the polyacrylonitrile mixed solution to a 5mL syringe equipped with a 20G needle, and use a microflow pump to uniformly add it to the anhydrous ethanol solution at a speed of 10ml / h. After the reaction is completed, let it stand for 30min to remove the PVP molecules, and filter to obtain polyacrylonitrile resin of uniform size.

[0063] Weigh 1g of polyacrylonitrile resin into a 250ml single-necked flask, add 1.8g of hydroxylamine hydrochloride into the 250ml single-necked flask, add 200ml of water to dissolve the hydroxylamine hydrochloride to obtain a resin modified liquid; then add 1.04g of sodium hydroxide into the single-necked flask, after the sodium hydroxide is completely dissolved, weigh 1g of polyacrylonitrile resin into the flask, transfer the flask to a 60°C water bath, react for 120min at a certain stirring rate, after the reaction is completed, filter with a filter device, then rinse with pure water several times, after washing, put the obtained material into anhydrous ethanol for dispersion for 30min, filter after dispersion, and finally put the material into a freeze dryer for drying to obtain amidoxime polyacrylonitrile resin material.

[0064] The obtained amidoxime polyacrylonitrile resin material was used to recover gallium ions from vanadium sludge acid leaching solution. The grafting rate of porous material groups was 85%, and the BET was 11.86m 2 / g, average particle size is 2.40mm, adsorption capacity is 46.48mg / g, see Figure 4 .

[0065] Example 3

[0066] Weigh 1.5g PAN (Da = 150000) powder and 3.5g PVP powder in a 25mL beaker, add 20mL DMF solution to the beaker, and heat and dissolve in a water bath with magnetic stirring until the solution is clear and transparent. Transfer the polyacrylonitrile mixed solution to a 5mL syringe equipped with a 22G needle, and use a microflow pump to uniformly add it to the anhydrous ethanol solution at a speed of 10ml / h. After the reaction is completed, let it stand for 30min to remove the PVP molecules, and filter to obtain polyacrylonitrile resin of uniform size.

[0067] Weigh 1g of polyacrylonitrile resin and put it into a 250ml single-mouth flask, add 1.8g of hydroxylamine hydrochloride into the 250ml single-mouth flask, add 200ml of water to dissolve the hydroxylamine hydrochloride to obtain a resin modified liquid; then add 1.04g of sodium hydroxide into the single-mouth flask, after the sodium hydroxide is completely dissolved, weigh 1g of polyacrylonitrile resin and put it into the flask, transfer the flask to a 60°C water bath, react for 120min at a certain stirring rate, after the reaction is completed, filter with a filter device, and then rinse with pure water several times. After washing, put the obtained material into anhydrous ethanol for dispersion for 30min, filter after dispersion, and finally put the material into a freeze dryer for drying to obtain amidoxime polyacrylonitrile resin material.

[0068] The obtained amidoxime polyacrylonitrile resin material is used to recover gallium ions from vanadium sludge acid leaching liquid. Figure 5 , SEM image of amidoxime material after adsorption of gallium (AOPAN-Ga). The grafting rate of porous material groups is 70%, and the BET is 11.82m 2 / g, the average particle size is 1.93mm, and the adsorption capacity is 37.53mg / g.

[0069] Example 4

[0070] Weigh 1.5g PAN (Da = 150000) powder and 4.5g PVP powder in a 25mL beaker, add 20mL DMF solution to the beaker, and heat and dissolve in a water bath with magnetic stirring until the solution is clear and transparent. Transfer the polyacrylonitrile mixed solution to a 5mL syringe equipped with a 22G needle, and use a microflow pump to uniformly add it to the anhydrous ethanol solution at a speed of 10ml / h. After the reaction is completed, let it stand for 30min to remove the PVP molecules, and filter to obtain polyacrylonitrile resin of uniform size.

[0071] Weigh 1g of polyacrylonitrile resin and put it into a 250ml single-mouth flask, add 1.2g of hydroxylamine hydrochloride into the 250ml single-mouth flask, add 200ml of water to dissolve the hydroxylamine hydrochloride to obtain a resin modified liquid; then add 0.69g of sodium hydroxide into the single-mouth flask, after the sodium hydroxide is completely dissolved, weigh 1g of polyacrylonitrile resin and put it into the flask, transfer the flask to a 60°C water bath, react for 120min at a certain stirring rate, after the reaction is completed, filter with a filter device, and then rinse with pure water several times. After washing, put the obtained material into anhydrous ethanol for dispersion for 30min, filter after dispersion, and finally put the material into a freeze dryer for drying to obtain amidoxime polyacrylonitrile resin material.

[0072] The obtained amidoxime polyacrylonitrile resin material was used to recover gallium ions from vanadium sludge acid leaching solution. The grafting rate of porous material groups was 69.86%, and the BET was 13.52m 2 / g, the average particle size is 1.96mm, and the adsorption capacity is 39.48mg / g.

[0073] Example 5

[0074] Weigh 1.5g PAN (Da = 150000) powder and 3.5g PVP powder in a 25mL beaker, add 20mL DMF solution to the beaker, and heat and dissolve in a water bath with magnetic stirring until the solution is clear and transparent. Transfer the polyacrylonitrile mixed solution to a 5mL syringe equipped with a 20G needle, and use a microflow pump to uniformly add it to the anhydrous ethanol solution at a speed of 10ml / h. After the reaction is completed, let it stand for 30min to remove the PVP molecules, and filter to obtain polyacrylonitrile resin of uniform size.

[0075] Weigh 1g of polyacrylonitrile resin and put it into a 250ml single-mouth flask, add 2.4g of hydroxylamine hydrochloride into the 250ml single-mouth flask, add 200ml of water to dissolve the hydroxylamine hydrochloride to obtain a resin modified liquid; then add 1.40g of sodium hydroxide into the single-mouth flask, after the sodium hydroxide is completely dissolved, weigh 1g of polyacrylonitrile resin and put it into the flask, transfer the flask to a 60°C water bath, react for 120min at a certain stirring rate, after the reaction is completed, filter with a filter device, and then rinse with pure water several times. After washing, put the obtained material into anhydrous ethanol for dispersion for 30min, filter after dispersion, and finally put the material into a freeze dryer for drying to obtain amidoxime polyacrylonitrile resin material.

[0076] The obtained amidoxime polyacrylonitrile resin material was used to recover gallium ions from the acid leaching solution of vanadium sludge. The grafting rate of porous material groups was 96.75%, and the BET was 11.79m 2 / g, the average particle size is 2.40mm, and the adsorption capacity is 55.68mg / g.

[0077] Figure 6 Infrared spectra of polyacrylonitrile powder, polyvinyl pyrrolidone, polyacrylonitrile resin, and amidoxime polyacrylonitrile resin in Example 5 of the present invention; Figure 7 is the infrared spectrum of AOPAN before and after adsorption of gallium in Example 5 of the present invention; Figure 6 and Figure 7 It can be seen that after the modification of polyacrylonitrile resin, the -1 The -C≡N peak is weakened and located at 1600cm -1 The vibration of the C=N peak at 943 cm -1 The NO peak at 598 cm- 1 The Ga-O peak at .

[0078] It can be seen from the above embodiments that the present invention provides a method for preparing amidoxime material using microfluidics, comprising the following steps: 1) mixing polyacrylonitrile powder, porogen and organic solvent to obtain a polyacrylonitrile solution; 2) absorbing the polyacrylonitrile solution, and controlling the polyacrylonitrile solution to be added to the solvent by microfluidics to obtain a polyacrylonitrile resin of uniform size; 3) mixing the polyacrylonitrile resin with water and hydroxylamine reagent, dissolving to obtain a resin modified liquid; 4) adjusting the pH value of the resin modified liquid, reacting, filtering to obtain a porous material; 5) dispersing, filtering and drying the porous material to obtain an amidoxime material. The amidoxime material prepared by the method has a high adsorption capacity for gallium. The group grafting rate of the amidoxime polyacrylonitrile resin material prepared by the method provided by the present invention is 68-97%; the BET of the amidoxime polyacrylonitrile resin material is 11.7-13.6m 2 / g; the average particle size of the amidoxime polyacrylonitrile resin material is 1.9 to 2.4 mm.

[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing amidoxime polyacrylonitrile resin material by microfluidics, comprising the following steps: 1) mixing polyacrylonitrile powder, a porogen and an organic solvent to obtain a polyacrylonitrile solution; 2) absorbing the polyacrylonitrile solution, and adding the polyacrylonitrile solution to the solvent by microfluidics to obtain polyacrylonitrile resin with uniform size; 3) mixing the polyacrylonitrile resin, water and hydroxylamine reagent, dissolving them, and obtaining a resin modified liquid; 4) adjusting the pH value of the resin modified liquid, reacting, filtering, and obtaining a porous material; 5) dispersing, filtering and drying the porous material to obtain amidoxime polyacrylonitrile resin material.

2. The method according to claim 1, characterized in that The flow rate of the microfluidic method in step 2) is 5 to 20 mL / min.

3. The method according to claim 1, characterized in that The molecular weight of the polyacrylonitrile powder in step 1) is 150,000 to 1,000,000; The porogen is one or more of polyvinyl pyrrolidone, sucrose, sodium chloride and polyethylene glycol; The organic solvent is selected from one or more of N'N-dimethylformamide, N'N-dimethylacetamide, dimethyl sulfoxide, isopropyl acetate and tetrahydrofuran.

4. The method according to claim 1, characterized in that: The reagent in step 2) is pure water, alcohol or an alcohol-water mixture.

5. The method according to claim 1, characterized in that In the step 3), the mass ratio of the liquid volume to the solid material in the resin modification liquid is (5-20) mL:1 g; The molar ratio of the hydroxylamine to the polyacrylonitrile is 1:1 to 4:

1.

6. The method according to claim 1, characterized in that In the step 4), a solid base is used to adjust the pH value; The solid alkali is selected from one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, potassium bicarbonate, sodium bicarbonate and ammonium bicarbonate.

7. The method according to claim 1, characterized in that In the step 4), the reaction temperature is 50-90° C. and the reaction time is 2-6 hours.

8. The method according to claim 1, characterized in that In the step 5), the porous material is dispersed using anhydrous ethanol for a dispersion time of 10 to 60 minutes; The drying temperature is -40℃~0℃, and the drying time is 6~12h.

9. Use of the amidoxime polyacrylonitrile resin material prepared by the method according to any one of claims 1 to 8 in recovering gallium ions from vanadium-extracting sludge acid leaching liquid.

Citation Information

Cited By

  • Gallium ion imprinted amidoxime-based macroporous resin as well as preparation method and application thereof