Sugar-grafted modified maleic anhydride alternating copolymer as well as preparation method and application thereof

By simplifying the synthesis of alternating copolymers of sugar graft modified maleic anhydride, the problems of complexity and low yield of anti-freeze glycoprotein synthesis are solved, and the ice nucleation temperature is improved and the ice crystal morphology is controlled. It is suitable for cell freezing Save and preserve protein.

CN118930703AInactive Publication Date: 2024-11-12TIANJIN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411181513.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing anti-freeze glycoprotein synthesis process is complex, with low yields and easy introduction of impurities. The modified zwitterionic polymer has weak control over the morphology of ice crystals.

Method used

By simplifying the synthesis method, sugar graft modification is prepared by combining commercially used methylvinyl ether-maleic anhydride or styrene-maleic anhydride alternating copolymers with sugars such as glucose, trehalose, maltose, and malttriose to prepare sugar graft modification using commercially available methyl vinyl ether-maleic anhydride or styrene-maleic anhydride alternating copolymers with glucose, trehalose, maltose, and maltaceous to prepare Maleic anhydride alternating copolymers, using mild reaction conditions and specific formulations and treatment steps, improve ice nucleation temperature and ice crystal morphology control capabilities.

Benefits of technology

The efficient preparation of sugar-grafted modified maleic anhydride alternating copolymer was achieved, which significantly increased the ice nucleation temperature of the solution and had strong control over the ice crystal morphology. It was suitable for cell freezing and long-term protein preservation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930703A_ABST
    Figure CN118930703A_ABST
Patent Text Reader

Abstract

The invention relates to a sugar-grafted modified maleic anhydride alternating copolymer as well as a preparation method and application thereof. The preparation method comprises the following steps: putting a methyl vinyl ether-maleic anhydride alternating copolymer or a styrene-maleic anhydride alternating copolymer and one of glucose, trehalose, maltose, maltotriose and pinotriose into a reaction container, introducing nitrogen into the bottle, adding anhydrous N, N-dimethylformamide, adding anhydrous triethylamine, reacting at 80-100 DEG C for 12-48 hours, cooling to room temperature, filtering, washing and drying to obtain the methyl vinyl ether-maleic anhydride copolymer. And precipitating the product in diethyl ether, dissolving with water, dialyzing in a dialysis bag with a large amount of water for 24-96 hours, and freeze-drying the dialyzed solution to obtain the sugar-grafted modified maleic anhydride alternating copolymer. The sugar-grafted modified maleic anhydride alternating copolymer is applied to control of ice crystal growth and control of ice crystal morphology in the form of an aqueous solution. The synthesis and purification method is simple and easy to operate, and reaction conditions are mild; the method has potential value in long-term preservation of protein and cell cryopreservation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sugar graft modification of maleic anhydride alternating copolymers and application of their ice control performance, and specifically relates to sugar graft modified maleic anhydride alternating copolymers and a preparation method and application thereof. Background Art

[0002] Carbohydrates have a polyhydroxy structure, including monosaccharides, disaccharides, trisaccharides, oligosaccharides and polysaccharides. High molecular weight polysaccharides extracted from birch seeds can promote ice nucleation, while low molecular weight polysaccharides can control the morphology of ice crystals, presenting a six-petal flower shape (Dreischmeier K, Budke C, Wiehemeier L. Sci. Rep. 2017, 7, 41890). In addition, antifreeze glycoproteins produced in microorganisms under extreme conditions in nature can inhibit the growth of ice crystals, thereby preventing tissue damage in cold climates. Inspired by antifreeze glycoproteins, glycopeptide polymers that combine small molecule sugars with polymers can achieve ice control functions. Kramer et al. synthesized an antifreeze glycoprotein-like polymer by ring-opening polymerization of sugar-modified N-carboxyl-α-amino acid anhydride. This polymer can control the growth of round ice crystals into hexagons, showing the ability to control the morphology of ice crystals (Deleray AC, Saini S, Wallberg AC, Kramer JR. Chem. Mater. 2024, 36, 3424-3434). However, the synthesis process of this antifreeze glycoprotein-like polymer is complicated, the yield is low, and the risk of introducing impurities is increased. The polymer directly modified by sugar can have a simple reaction step, which increases the yield while also reducing the risk of introducing more impurities. Gao Shuhui et al. prepared glucose, trehalose, maltose and maltotriose grafted polylysine by amidation method. The synthesized glycopeptide had an ice recrystallization inhibition activity of 26% relative to hydroxyethylpiperazineethanesulfonic acid buffer solution (Gao S, Zhu K, Zhang Q, Niu Q, Chong J, Ren L, Yuan X. Biomacromolecules 2022, 23, 530-542).

[0003] Maleic anhydride alternating copolymer is an alternating copolymer formed by the alternating copolymerization of maleic anhydride monomer and vinyl monomer. The synthesis process of methyl vinyl ether-maleic anhydride alternating copolymer and styrene-maleic anhydride alternating copolymer is very mature and is a commercial product. The product modification can be achieved through the chemical reaction of maleic anhydride groups. British scholar Gibson et al. imitated the structure of natural antifreeze protein and obtained a zwitterionic polymer with both amino and carboxyl groups in the side chain by modifying methyl vinyl ether-maleic anhydride alternating copolymer with ethanolamine. This polymer has a concentration of 20mg·mL -1It has ice recrystallization inhibition activity, and the average maximum ice crystal size produced is 20% of that of phosphate buffer solution (Mitchell DE, Cameron NR, Gibson MI. Chem. Commun. 2015, 51, 12977-12980), and has potential applications in cell cryopreservation (Bailey TL, Stubbs C, Murray K, Tomas RM, Otten L, Gibson MI. Biomacromolecules 2019, 20, 3104-3114). However, based on the difference in the structure of antifreeze protein and antifreeze glycoprotein itself, the modified zwitterionic polymer has a weak effect on ice crystal morphology.

[0004] Inspired by antifreeze glycoproteins, the synthesis method of maleic anhydride alternating copolymers modified by direct grafting of sugars can obtain sugar-grafted maleic anhydride alternating copolymers with both sugar and carboxyl groups on the side chains. Due to the biomimetic structure of natural antifreeze glycoproteins, the aqueous solution of sugar-grafted maleic anhydride alternating copolymers can be used to control the morphology of ice crystals, and significantly promote ice nucleation, increase the freezing temperature of the solution, and have potential value in long-term protein storage and cell cryopreservation. The preparation conditions of sugar-grafted maleic anhydride alternating copolymers are mild, and there are no reports on the synthesis and application of sugar-modified maleic anhydride alternating copolymers. Summary of the invention

[0005] The present invention aims to imitate the structure of natural antifreeze glycoproteins, obtain an alternating copolymer with rich sugars in the side chains with strong universality through simple and easy synthesis and mild reaction conditions. The obtained sugar-grafted modified maleic anhydride alternating copolymer not only has a controlling effect on the morphology of ice crystals, but also can significantly increase the ice nucleation temperature of the solution.

[0006] The invention uses commercially available methyl vinyl ether-maleic anhydride alternating copolymer or styrene-maleic anhydride alternating copolymer and one of glucose, trehalose, maltose, maltotriose and melezitose as raw materials to prepare sugar-grafted modified maleic anhydride alternating copolymer.

[0007] The technical purpose of the present invention is achieved through the following scheme:

[0008] A sugar grafted modified maleic anhydride alternating copolymer, the chemical structure of which is as follows:

[0009] The value of n is 9 to 833, the side group R1 is CH3O- or -C6H5; the molecular weight of the obtained sugar grafted modified maleic anhydride alternating copolymer is 3500 to 550,000.

[0010] R2 is

[0011]

[0012] The preparation method of sugar graft modified maleic anhydride alternating copolymer is as follows:

[0013] A methyl vinyl ether-maleic anhydride alternating copolymer or a styrene-maleic anhydride alternating copolymer and one of glucose, trehalose, maltose, maltotriose and melezitose are placed in a reaction container, anhydrous N,N-dimethylformamide is added after nitrogen is introduced into the bottle, anhydrous triethylamine is added, and the reaction is carried out at 80-100° C. for 12-48 hours, the product is precipitated in ether and then dissolved in water, and then dialyzed in a dialysis bag with a large amount of water for 24-96 hours, and the solution obtained after dialysis is freeze-dried to obtain a sugar-grafted modified maleic anhydride alternating copolymer.

[0014] The molar ratio of the anhydride group to one of glucose, trehalose, maltose, maltotriose and melezitose in the maleic anhydride alternating copolymer is 1:(2-5);

[0015] The addition of anhydrous N,N-dimethylformamide makes the molar concentration of the anhydride groups contained in the maleic anhydride alternating copolymer range from 50 to 100 mmol·L -1 .

[0016] The volume ratio of the added anhydrous triethylamine to anhydrous N,N-dimethylformamide is 1:(100-300).

[0017] The dialysis time is 24 to 96 hours, and the molecular weight cutoff of the dialysis bag is in the range of 500 to 20,000.

[0018] The sugar graft modified maleic anhydride alternating copolymer of the present invention is used in the form of aqueous solution to control ice crystal growth and ice crystal morphology.

[0019] The present invention also discloses a method for observing the control of the morphology of ice crystals by sugar-grafted modified maleic anhydride alternating copolymer in a sucrose aqueous solution, wherein the temperature is controlled to increase so that only a small amount of ice crystals remain in the frozen solution during the annealing process, and then the temperature is lowered to record the morphology of ice crystals formed after the ice crystals grow for 40 minutes. In addition, a method for observing the ice nucleation temperature determined by the freezing of half of the microliter droplets is also disclosed, and the ice nucleation temperature of pure water is measured to be -22.2°C, which is compared with the ice nucleation temperature of pure water.

[0020] The advantages of the present invention are that the synthesis and purification method for preparing the sugar-grafted modified maleic anhydride alternating copolymer is simple and easy to operate, and the reaction conditions are mild; the raw materials are commercially available maleic anhydride alternating copolymer and sugar, which can be mass-produced and used in large quantities; the prepared sugar-grafted modified maleic anhydride alternating copolymer has strong water solubility, which is convenient for the use of polymer solutions. The sugar-grafted modified maleic anhydride alternating copolymer can significantly increase the ice nucleation temperature of the solution, and has a control effect on the morphology of ice crystal formation, and has potential value for application in cell cryopreservation and long-term storage of proteins. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 :Glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer's control effect on ice crystal morphology (a) and its effect of promoting ice nucleation (b)

[0022] Figure 2 :The control effect of trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer on ice crystal morphology (a) and the effect of promoting ice nucleation (b)

[0023] Figure 3 :The effect of melezitose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer on the control of ice crystal morphology (a) and the promotion of ice nucleation (b) DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below through implementation cases. The following specific implementation cases are further descriptions of the present invention, but do not limit the scope of application of the present invention.

[0025] Embodiment 1:

[0026] Preparation of glucose grafted modified styrene-maleic anhydride alternating copolymer:

[0027] 1.30 g of glucose and 0.65 g of styrene-maleic anhydride alternating copolymer (n=9), i.e., the molar ratio of anhydride to glucose in the styrene-maleic anhydride alternating copolymer was 1:2, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 50 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 60 mmol·L -1 After the solid was completely dissolved, 0.2 mL of anhydrous triethylamine was added to the bottle and reacted at 80°C for 48 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved in water, the solution was placed in a dialysis bag with a molecular weight cutoff of 500 and dialyzed with a large amount of water for 48 hours. After freeze-drying, glucose-grafted modified styrene-maleic anhydride alternating copolymer was obtained.

[0028] The structure of the glucose grafted modified styrene-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 3500.

[0029]

[0030] Embodiment 2:

[0031] Preparation of trehalose grafted modified styrene-maleic anhydride alternating copolymer:

[0032] 2.46 g of trehalose and 0.65 g of styrene-maleic anhydride alternating copolymer (n=9), i.e., the molar ratio of anhydride to trehalose in the styrene-maleic anhydride alternating copolymer was 1:3, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 60 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 50 mmol·L -1 After the solid was completely dissolved, 0.2 mL of anhydrous triethylamine was added to the bottle and reacted at 80°C for 48 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved with water, the solution was placed in a dialysis bag with a molecular weight cutoff of 500 and dialyzed with a large amount of water for 48 hours. After freeze-drying, trehalose-grafted modified styrene-maleic anhydride alternating copolymer was obtained.

[0033] The structure of the trehalose graft-modified styrene-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 5,000.

[0034]

[0035] Embodiment 3:

[0036] Preparation of glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer:

[0037] 1.72 g of glucose and 0.5 g of methyl vinyl ether-maleic anhydride alternating copolymer (n=513), i.e., the molar ratio of anhydride to glucose in the methyl vinyl ether-maleic anhydride alternating copolymer was 1:3, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 30 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 100 mmol·L -1 After the solid was completely dissolved, 0.1 mL of anhydrous triethylamine was added to the bottle and reacted at 80°C for 12 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved in water, the solution was placed in a dialysis bag with a molecular weight cutoff of 1,000 and dialyzed with a large amount of water for 24 hours. After freeze-drying, glucose-grafted modified methyl vinyl ether-maleic anhydride alternating copolymer was obtained.

[0038] The structure of the glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 170,000.

[0039]

[0040] Embodiment 4:

[0041] Preparation of glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer:

[0042] 1.15 g of glucose and 0.5 g of methyl vinyl ether-maleic anhydride alternating copolymer (n=833), i.e., the molar ratio of anhydride to glucose in the methyl vinyl ether-maleic anhydride alternating copolymer was 1:2, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 30 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 100 mmol·L -1 After the solid was completely dissolved, 0.3 mL of anhydrous triethylamine was added to the bottle and reacted at 80°C for 24 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved in water, the solution was placed in a dialysis bag with a molecular weight cutoff of 3,500 and dialyzed with a large amount of water for 24 hours. After freeze-drying, glucose-grafted modified methyl vinyl ether-maleic anhydride alternating copolymer was obtained.

[0043] The structure of the glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 279,000.

[0044]

[0045] Embodiment 5:

[0046] Preparation of trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer:

[0047] 3.28 g of trehalose and 0.5 g of methyl vinyl ether-maleic anhydride alternating copolymer (n=513), i.e., the molar ratio of anhydride to trehalose in the methyl vinyl ether-maleic anhydride alternating copolymer was 1:3, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 50 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 60 mmol·L -1 After the solid was completely dissolved, 0.2 mL of anhydrous triethylamine was added to the bottle and reacted at 100°C for 48 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved in water, the solution was placed in a dialysis bag with a molecular weight cutoff of 2,000 and dialyzed with a large amount of water for 24 hours. After freeze-drying, trehalose-grafted modified methyl vinyl ether-maleic anhydride alternating copolymer was obtained.

[0048] The structure of the trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 257,000.

[0049]

[0050] Embodiment 6:

[0051] Preparation of maltose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer:

[0052] 3.28 g of maltose and 0.5 g of methyl vinyl ether-maleic anhydride alternating copolymer (n=513), i.e., the molar ratio of anhydride to maltose in the methyl vinyl ether-maleic anhydride alternating copolymer was 1:3, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 50 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 60 mmol·L -1 After the solid was completely dissolved, 0.2 mL of anhydrous triethylamine was added to the bottle and reacted at 90°C for 48 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved in water, the solution was placed in a dialysis bag with a molecular weight cutoff of 2,000 and dialyzed with a large amount of water for 24 hours. After freeze-drying, maltose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer was obtained.

[0053] The structure of the maltose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 257,000.

[0054]

[0055] Embodiment 7:

[0056] Preparation of trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer:

[0057] 2.19 g of trehalose and 0.5 g of methyl vinyl ether-maleic anhydride alternating copolymer (n=833), i.e., the molar ratio of anhydride to trehalose in the methyl vinyl ether-maleic anhydride alternating copolymer was 1:2, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 50 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 60 mmol·L -1 After the solid was completely dissolved, 0.2 mL of anhydrous triethylamine was added to the bottle and reacted at 90°C for 48 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved with water, the solution was placed in a dialysis bag with a molecular weight cutoff of 20,000 and dialyzed with a large amount of water for 48 hours. After freeze-drying, trehalose-grafted modified methyl vinyl ether-maleic anhydride alternating copolymer was obtained.

[0058] The structure of the trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 417,000.

[0059]

[0060] Embodiment 8:

[0061] Preparation of maltotriose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer:

[0062] 4.84 g of maltotriose and 0.5 g of methyl vinyl ether-maleic anhydride alternating copolymer (n=513), i.e., the molar ratio of anhydride to maltotriose in the methyl vinyl ether-maleic anhydride alternating copolymer was 1:5, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 30 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 100 mmol·L -1 After the solid was completely dissolved, 0.1 mL of anhydrous triethylamine was added to the bottle and reacted at 90°C for 48 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved with water, the solution was placed in a dialysis bag with a molecular weight cutoff of 20,000 and dialyzed with a large amount of water for 96 hours. After freeze-drying, maltotriose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer was obtained.

[0063] The structure of the maltotriose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 339,000.

[0064]

[0065] Embodiment 9:

[0066] Preparation of maltotriose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer:

[0067] 3.23 g of maltotriose and 0.5 g of methyl vinyl ether-maleic anhydride alternating copolymer (n=833), i.e., the molar ratio of anhydride to maltotriose contained in the methyl vinyl ether-maleic anhydride alternating copolymer was 1:2, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 40 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 75 mmol·L -1 After the solid was completely dissolved, 0.2 mL of anhydrous triethylamine was added to the bottle and reacted at 80°C for 48 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved with water, the solution was placed in a dialysis bag with a molecular weight cutoff of 2,000 and dialyzed with a large amount of water for 48 hours. After freeze-drying, maltotriose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer was obtained.

[0068] The structure of the maltotriose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 550,000.

[0069]

[0070] Embodiment 10:

[0071] Preparation of melezitose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer:

[0072] 4.84 g melezitose and 0.5 g methyl vinyl ether-maleic anhydride alternating copolymer (n=833), i.e., the molar ratio of anhydride to melezitose in the methyl vinyl ether-maleic anhydride alternating copolymer was 1:3, were placed in a 100 mL Shrek bottle. After nitrogen was introduced into the bottle, 50 mL of anhydrous N,N-dimethylformamide was added to the system. At this time, the molar concentration of the anhydride was 60 mmol·L -1 After the solid was completely dissolved, 0.2 mL of anhydrous triethylamine was added to the bottle and reacted at 100°C for 48 hours. After the reaction, the product was precipitated in ether and filtered. After being dissolved with water, the solution was placed in a dialysis bag with a molecular weight cutoff of 3500 and dialyzed with a large amount of water for 48 hours. After freeze-drying, a melezitose-grafted modified methyl vinyl ether-maleic anhydride alternating copolymer was obtained.

[0073] The structure of the melezitose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained by the above reaction is shown below, and the molecular weight is 525,000.

[0074]

[0075] Embodiment 11:

[0076] The glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained in Example 4 was dissolved in a sucrose aqueous solution with a mass fraction of 40% to make the concentration of the glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer 10 mg·mL -1 , take 1 μl and drop it in the center of the circular cover glass, cover it with another cover glass of the same size, move it to the cold stage, and first cool it at 30℃·min -1 The cooling rate was 5℃·min -1 The temperature was raised to -8°C at a rate of 0.05°C / min. -1 The temperature was raised at a rate of 0.05°C·min until only a small amount of ice crystals remained on the sample. -1- Cool down for 40 minutes and take photos to record the morphology of the ice crystals formed, such as Figure 1As shown in (a), comb-shaped ice crystals are formed, indicating that glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer has a controlling effect on the morphology of ice crystals.

[0077] Embodiment 12:

[0078] The trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained in Example 7 was dissolved in a 40% sucrose aqueous solution to make the concentration of the trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer 10 mg mL -1 , take 1 μl and drop it in the center of the circular cover glass, cover it with another cover glass of the same size, move it to the cold stage, and first cool it at 30℃·min -1 The cooling rate was 5℃·min -1 The temperature was raised to -8°C at a rate of 0.05°C / min. -1 The temperature was raised at a rate of 0.05°C·min until only a small amount of ice crystals remained on the sample. -1- Cool down for 40 minutes and take photos to record the morphology of the ice crystals formed, such as Figure 2 As shown in (a), dendritic ice crystals are formed, indicating that trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer has a controlling effect on the morphology of ice crystals.

[0079] Embodiment 13:

[0080] The melezitose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained in Example 10 was dissolved in a sucrose aqueous solution having a mass fraction of 40% to make the concentration of the melezitose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer 10 mg·mL -1 , take 1 μl and drop it in the center of the circular cover glass, cover it with another cover glass of the same size, move it to the cold stage, and first cool it at 30℃·min -1 The cooling rate was 5℃·min -1 The temperature was raised to -8°C at a rate of 0.05°C / min. -1 The temperature was raised at a rate of 0.05°C·min until only a small amount of ice crystals remained on the sample. -1- Cool down for 40 minutes and take photos to record the morphology of the ice crystals formed, such as Figure 3 As shown in (a), dendritic ice crystals are formed, indicating that the melezitose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer has a controlling effect on the morphology of ice crystals.

[0081] Embodiment 14:

[0082] The glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained in Example 4 was prepared into 10 mg·mL -1 Arrange 20 0.8 μL droplets of aqueous solution on an iron sheet and place them on a cold stage. -1 The temperature of the cold stage was lowered to 5°C at a rate of 1°C min-1 and maintained for 3 minutes. -1 The temperature of the cold stage was lowered at a rate of 100 μg / mL and the temperature at which each droplet became opaque was recorded. The temperature at which half of the droplets became opaque was designated as 10 mg / mL -1 The nucleation temperature of trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer. Figure 1 As shown in (b), the ice nucleation temperature is increased by 10.6°C compared with that of pure water, proving that the glucose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer has the effect of significantly increasing the ice nucleation temperature.

[0083] Embodiment 15:

[0084] The trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained in Example 7 was prepared into 10 mg·mL -1 Arrange 20 0.8 μL droplets of aqueous solution on an iron sheet and place them on a cold stage. -1 The temperature of the cold stage was lowered to 5°C at a rate of 1°C min-1 and maintained for 3 minutes. -1 The temperature of the cold stage was lowered at a rate of 100 μg / mL and the temperature at which each droplet became opaque was recorded. The temperature at which half of the droplets became opaque was designated as 10 mg / mL -1 The nucleation temperature of trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer. Figure 2 As shown in (b), the ice nucleation temperature is increased by 10.0℃ compared with that of pure water, which proves that the trehalose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer has the effect of significantly increasing the ice nucleation temperature.

[0085] Embodiment 16:

[0086] The melezitose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer obtained in Example 10 was prepared into 10 mg·mL -1 Arrange 20 0.8 μL droplets of aqueous solution on an iron sheet and place them on a cold stage. -1 The temperature of the cold stage was lowered to 5°C at a rate of 1°C min-1 and maintained for 3 minutes. -1 The temperature of the cold stage was lowered at a rate of 100 μg / mL and the temperature at which each droplet became opaque was recorded. The temperature at which half of the droplets became opaque was designated as 10 mg / mL -1 The nucleation temperature of melezitose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer. Figure 3 As shown in (b), the ice nucleation temperature is increased by 11.0°C compared with that of pure water, proving that the melezitose grafted modified methyl vinyl ether-maleic anhydride alternating copolymer has the effect of significantly increasing the ice nucleation temperature.

[0087] The preparation method of a sugar-modified maleic anhydride alternating copolymer disclosed and proposed in the present invention and its application in ice control can be realized by those skilled in the art by referring to the content of this article and appropriately changing the conditions, routes and other links. Although the method of the present invention has been described through preferred embodiments, relevant technicians can obviously modify or recombine the methods and technical routes described herein without departing from the spirit, scope and content of the present invention to achieve the final preparation technology. It should be particularly pointed out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the spirit, scope and content of the present invention.

Claims

1. A sugar grafted modified maleic anhydride alternating copolymer, characterized in that: The chemical structure is as follows: Wherein, R1=CH3O-, -C6H5; 2. The sugar grafted modified maleic anhydride alternating copolymer according to claim 1, characterized in that: The maleic anhydride alternating copolymer is a methyl vinyl ether-maleic anhydride alternating copolymer or a styrene-maleic anhydride alternating copolymer.

3. The sugar grafted modified maleic anhydride alternating copolymer according to claim 1, characterized in that: The value of n is 9 to 833, and the molecular weight of the sugar-modified maleic anhydride alternating copolymer is 3,500 to 550,000.

4. The method for preparing the sugar-grafted modified maleic anhydride alternating copolymer according to claim 1, characterized in that: The maleic anhydride alternating copolymer and one of glucose, trehalose, maltose, maltotriose or melezitose are placed in a reaction container, anhydrous N,N-dimethylformamide and anhydrous triethylamine are added after nitrogen is introduced into the bottle, and the reaction is stirred at 80-100° C. for 12-96 hours, the product is precipitated in ether and then dissolved in water, and the solution obtained after water dialysis is freeze-dried to obtain the sugar-grafted modified maleic anhydride alternating copolymer.

5. The method for synthesizing the sugar-grafted modified maleic anhydride alternating copolymer according to claim 4, characterized in that: The molar ratio of the anhydride group to one of glucose, trehalose, maltose, maltotriose and melezitose in the maleic anhydride alternating copolymer is 1:(2-5).

6. The method for synthesizing the sugar-grafted modified maleic anhydride alternating copolymer according to claim 4, characterized in that: Anhydrous N,N-dimethylformamide was added to make the molar concentration of the anhydride groups in the maleic anhydride alternating copolymer range from 50 to 100 mmol·L -1 .

7. The method for synthesizing the sugar-grafted modified maleic anhydride alternating copolymer as claimed in claim 4, characterized in that: The volume ratio of anhydrous triethylamine to anhydrous N,N-dimethylformamide added is 1:(100-300).

8. The method for synthesizing the sugar-grafted modified maleic anhydride alternating copolymer according to claim 4, characterized in that: The dialysis time is 24 to 96 hours, and the molecular weight cutoff of the dialysis bag ranges from 500 to 20,000.

9. The sugar-grafted modified maleic anhydride alternating copolymer according to claim 1 is used in the form of aqueous solution to control ice crystal growth and ice crystal morphology.

Citation Information

Patent Citations

  • Application of cyclodextrin-methyl vinyl ether / maleic anhydride copolymer and self-assembled nanoparticle of copolymer in oral medicine delivery

    CN104387592A

  • Polysaccharide microspheres, preparation method thereof and adsorption column

    CN115779875A