Preparation method and application of water-based conductive binder for silicon-based negative electrode of lithium ion battery

By preparing a thermally self-crosslinking aqueous conductive binder, the problem of electrode damage caused by volume expansion of silicon-based anode materials was solved, improving the cycle performance and environmental friendliness of lithium-ion batteries, and realizing the application of highly efficient silicon-based anode materials.

CN118930710AActive Publication Date: 2024-11-12SOUTH CHINA UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410901699.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-12
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

Existing silicon-based anode materials suffer from electrode damage and reduced cycle performance in lithium-ion batteries due to volume expansion. Furthermore, traditional binders use organic solvents, which are harmful to the environment and costly, making them difficult to meet industrial requirements.

Method used

A method for preparing an aqueous conductive adhesive using thermal self-crosslinking and in-situ network structure formed by silicon particles is employed. This method enhances the ionic conductivity and strong adhesion of the adhesive by introducing functional monomers, thereby reducing the amount of adhesive used. Monomer A is neutralized with lithium hydroxide, and carbodiimide hydrochloride and N-hydroxysuccinimide are added for polymerization to form multiple hydrogen bonds.

Benefits of technology

It improves the initial coulombic efficiency and cycle performance of lithium-ion batteries, reduces the impact of silicon volume expansion, enhances battery stability and capacity, reduces environmental harm, and the process is simple and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930710A_ABST
    Figure CN118930710A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a water-based conductive binder for a silicon-based negative electrode of a lithium ion battery. The water-based conductive adhesive provided by the invention is a multi-component copolymerized polymer aqueous solution, and the polymer aqueous solution is prepared by copolymerizing a monomer A, a monomer B and a monomer C in water and then carrying out grafting reaction with a sulfamate monomer D containing a long-chain ether bond. The solid content of the obtained solution is 2.5-5% after dialysis and purification, and the solution has the characteristics of water solubility, thermal crosslinking and ionic conductivity enhancement, and solves the problems of large viscosity and difficult dispersion of the cross-linked network binder slurry. According to the present invention, the electrode material coated on the copper foil has characteristics of strong dry-wet adhesion and difficult shedding, the binder is used for the silicon-based negative electrode so as to alleviate the influence of silicon volume expansion, and the battery has characteristics of high specific capacity and good cycle performance. The method has the advantages of low cost, simplicity, universality, environment friendliness, good coating effect and the like, and is suitable for the silicon-based negative electrode of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a preparation method and application of a lithium ion battery silicon-based negative electrode aqueous conductive binder. Background Art

[0002] Lithium-ion batteries have the advantages of high energy efficiency, high power density, light weight and environmental friendliness, and have been widely used in electronic devices such as mobile phones, laptops and digital cameras. However, with the development of electric vehicles and emerging technologies of artificial intelligence, lithium-ion batteries need to have higher energy density while ensuring safety. The negative electrode material plays a vital role in the energy density and performance of lithium-ion batteries. At present, graphite negative electrode is the most widely used negative electrode material. The theoretical specific capacity of graphite is only 372mAh·g -1 , and as the graphite industry matures, the actual specific capacity of high-end graphite products is very close to the theoretical value. Silicon has a specific capacity of 3579 mAh g at room temperature. -1 In addition, silicon negative electrode materials also have the advantages of low electrochemical potential, high safety and environmental friendliness during lithiation and delithiation. Therefore, silicon is considered to be very promising to replace traditional graphite negative electrode materials as the negative electrode material of the next generation of high energy density lithium-ion batteries in the future.

[0003] Silicon negative electrode materials will produce up to 300% volume expansion during the lithium insertion process, which seriously damages the integrity of the electrode and leads to rapid attenuation of the silicon negative electrode capacity. Possible reasons for the failure of silicon negative electrode materials are: (1) The formation of an unstable and thick solid electrolyte interface (SEI). The drastic change in silicon volume during the lithium insertion process destroys the original SEI layer, causing silicon to be exposed on the surface and form a new SEI layer with the electrolyte. This process will continuously consume lithium ions and electrolytes, and eventually deplete the electrolyte. (2) Large volume changes lead to high internal stress on silicon particles, which in turn causes the material (active substances, etc.) to break and pulverize. (3) Peeling effect. The continuous volume change and pulverization of silicon negative electrode materials cause many active substances to lose their connection with the conductive network and current collector, resulting in the electrode layer peeling off from the current collector. At present, in order to solve the problem of decreased battery cycle performance caused by volume changes of silicon negative electrodes, the improvement methods include silicon material nano-silicon, composite materials, pre-lithiation technology and high-performance binders. The first three methods are costly and complex in process, while the development cost of high-performance binders is low and the method is simple. At the same time, the binder plays a vital role in the electrochemical properties of the electrode, which can reduce the impact of silicon volume expansion and improve the cycle performance of the battery.

[0004] So far, the scientific community has proposed a variety of working mechanisms of binders, which can be mainly divided into wetting theory, mechanical interlocking theory, chemical bonding theory, acid-base theory, diffusion theory, electrostatic theory and weak boundary layer theory. Among them, in lithium-ion battery binders, wetting theory, mechanical interlocking theory and chemical bonding theory are three theories widely used to explain the bonding between binders and active materials. From the perspective of wetting, it is hoped that the binder can completely wet the surface of the active material and the conductive additive, so as to achieve close contact between the binder and the adherend and reduce the generation of defects on the bonding interface. From the perspective of mechanical interlocking, in order to produce significant mechanical interlocking, it is necessary to increase the surface roughness and porosity of the electrode material, select a suitable bonding system, and prepare a binder solution with appropriate viscosity to ensure effective mixing and dispersion. From the perspective of chemical bonding theory, it is hoped that strong interactions such as hydrogen bonds, covalent bonds, and coordination bonds will be generated between the binder and the active material. Existing silicon-based negative electrode binders have the disadvantages of weak interaction with silicon, use of environmentally harmful organic solvents, large dosage, poor stability and poor cycle performance, which are difficult to meet industrial needs. Summary of the invention

[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing and applying a water-based conductive binder for silicon-based negative electrodes of lithium-ion batteries, thereby solving the problem of environmental damage caused by the need to use organic solvents to dissolve the binder; the effect of silicon volume expansion on battery cycle performance is reduced by forming a network structure with silicon particles in situ through thermal self-crosslinking; the ionic conductivity of the binder is enhanced by introducing functional monomers; and the strong adhesion of the binder can reduce the amount of binder used.

[0006] The purpose of the present invention is achieved through the following technical solutions.

[0007] A method for preparing a lithium-ion battery silicon-based negative electrode aqueous conductive binder comprises the following steps:

[0008] (1) dissolving lithium hydroxide in water, adding monomer A for neutralization, wherein the (carboxyl) neutralization degree is 60 to 80%; the monomer A is at least one of acrylic acid, methacrylic acid, maleic acid, and itaconic acid;

[0009] (2) mixing the neutralized solution in step (1) with monomer B, monomer C and water, adding an initiator solution to obtain a mixed solution, while passing a protective gas to remove oxygen, and then heating to 60 to 80° C. for reaction for 24 to 36 hours; the monomer B is at least one of hydroxyethyl acrylate, butyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate; and the monomer C is at least one of N-hydroxymethyl acrylamide, polyethylene glycol diacrylamide, and N-hydroxypropyl acrylamide;

[0010] (3) dissolving the polymer aqueous solution obtained in step (2) in a buffer solution, adding carbodiimide hydrochloride, N-hydroxysuccinimide and monomer D, and stirring the reaction for 9 to 12 hours; the monomer D is an aminosulfonate containing a long-chain ether bond;

[0011] (4) dialyzing the solution obtained in step (3) to obtain an aqueous conductive binder for a lithium-ion battery silicon-based negative electrode.

[0012] Preferably, in step (1), monomer A is added in a water bath at room temperature;

[0013] Preferably, in step (2), the protective gas is nitrogen.

[0014] Preferably, in step (2), the initiator is a combination of one or more of azobisisobutyronitrile, azobisisobutyramidine hydrochloride, ammonium persulfate, and potassium persulfate;

[0015] Preferably, in step (2), the mass of the initiator is 0.5 to 1% of the total mass of monomer A, monomer B, and monomer C;

[0016] Preferably, in step (2), the initiator solution is added in 3 to 4 times during the reaction.

[0017] Preferably, the mass percentage content of the monomer A, monomer B, and monomer C is 40-60% of monomer A, 20-40% of monomer B, and 10-20% of monomer C, and the sum of the mass percentages of monomer A, monomer B, and monomer C is 100%;

[0018] Preferably, in step (2), the ratio of the total mass of monomer A, monomer B, and monomer C in the mixed solution to the mass of water is (10-15):(90-85).

[0019] Preferably, in step (3), the buffer solution is a phosphate buffer solution; the pH of the buffer solution is 6.5-7; the dosage ratio of the polymer aqueous solution to the buffer solution is 50 g: (100-150) mL;

[0020] Preferably, in step (3), the total mass of the carbodiimide hydrochloride and N-hydroxysuccinimide (catalyst for grafting reaction) is 8-15% of the solid content in the polymer aqueous solution; the mass ratio of the carbodiimide hydrochloride and N-hydroxysuccinimide is (3-2):2.

[0021] Preferably, in step (3), the ratio of the molar amount of the monomer D to the molar amount of the carboxyl group of the monomer A is 40 to 60%.

[0022] Preferably, in step (3), the stirring reaction is carried out at room temperature.

[0023] Preferably, in step (3), the structural formula of the monomer D is as follows Figure 1 As shown, the average value of n is 6.

[0024] Preferably, in step (4), the dialysis bag is a 10-15 kDa dialysis bag; and the dialysis is performed 2-3 times.

[0025] A lithium ion battery silicon-based negative electrode aqueous conductive adhesive is prepared by the above-mentioned preparation method.

[0026] Preferably, the solid content of the aqueous conductive adhesive is 2.5-5%.

[0027] A lithium ion battery negative electrode plate comprises, by mass percentage, 80-90% of negative electrode active material, 5-10% of conductive agent, and 5-10% of aqueous binder, the sum of the mass percentages of each component being 100%; the aqueous binder is the above-mentioned lithium ion battery silicon-based negative electrode aqueous conductive binder.

[0028] Preferably, the negative electrode active material is a silicon-oxygen composite material or a silicon-carbon composite material;

[0029] Preferably, the conductive agent is at least one of conductive carbon black, acetylene black, graphene, conductive graphite, Ketjen black, super P, carbon nanotubes and conductive carbon fibers; and has the advantages of small particle size and good conductive properties.

[0030] Preferably, the negative electrode active material content of the negative electrode plate of the lithium ion battery is 1.2 to 2.0 mg·cm -2 .

[0031] A method for preparing a negative electrode sheet of a lithium ion battery comprises the following steps:

[0032] After the negative electrode active material, conductive agent, the above-mentioned lithium ion battery silicon-based negative electrode aqueous binder and water are mixed, they are fully ground to control the viscosity, and the slurry is coated on the copper foil with a scraper, placed in a 110-150°C oven for 3-5 hours, and then placed in a 60-80°C vacuum drying oven for 9-12 hours.

[0033] Preferably, the slurry viscosity is controlled at 1000-2000 mPa·s to achieve better coating effect.

[0034] Application of the above-mentioned lithium-ion battery silicon-based negative electrode aqueous conductive binder or the above-mentioned lithium-ion battery negative electrode plate in the preparation of lithium-ion batteries.

[0035] A method for preparing a lithium ion half-cell comprises the following steps:

[0036] In the glove box, place the lithium sheet on the negative electrode shell, add a diaphragm, drip the electrolyte, place the negative electrode sheet, gasket, and shrapnel in sequence, then add the positive electrode shell, and finally use a battery packaging machine to pressurize and seal.

[0037] Preferably, the electrolyte needs to contain fluoroethylene carbonate (FEC), which can enhance the cycle stability of the battery.

[0038] More preferably, the content of fluoroethylene carbonate (FEC) is 10%.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The aqueous conductive binder provided by the present invention can increase the molecular weight of the polymer by using lithium hydroxide to lithiation, while replenishing a small amount of lithium consumed by the negative electrode, further improving the initial coulombic efficiency.

[0041] (2) The aqueous conductive adhesive provided by the present invention contains a large number of functional groups with multiple hydrogen bonds that have strong interactions with silicon-based electrodes, which can reduce the impact of silicon volume expansion and improve the capacity and cycle performance of the battery.

[0042] (3) The aqueous conductive binder provided by the present invention can achieve thermal self-crosslinking, so that the viscosity of the slurry prepared will not be too high to be difficult to coat, thereby increasing the loading amount of the active material. At the same time, the network formed by thermal crosslinking can limit the expansion of the silicon volume, thereby reducing the effects of shedding, etc., and improving the stability and cycle performance of the battery.

[0043] (4) The aqueous conductive binder provided by the present invention can enhance the ionic conductivity of the binder by introducing aqueous aminosulfonate containing long-chain ether bonds into the side chain, thereby reducing the amount of conductive agent used, increasing the proportion of active materials, and increasing the battery capacity.

[0044] (5) The raw materials of the aqueous conductive adhesive provided by the present invention are easily available, no other organic solvents are used, the synthesis process is simple and environmentally friendly, and it has certain industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 is the structural formula of monomer D.

[0046] Figure 2 This is the reaction formula of the water-based binder in Example 1.

[0047] Figure 3 This is a flow chart for preparing the water-based binder of Example 1.

[0048] Figure 4 This is the infrared spectrum of the water-based binder of Example 1.

[0049] Figure 5aHalf-cell prepared with aqueous binder in Example 1 0.325A·g -1 Cycle performance diagram.

[0050] Figure 5b Half-cell 0.65A·g prepared by aqueous binders of Example 1, Comparative Example 1 and Comparative Example 2 -1 Cycle performance diagram.

[0051] Figure 6a and 6b The scanning electron microscope images of the electrode prepared with the aqueous binder in Example 1 before cycling and after 100 cycles are shown respectively. DETAILED DESCRIPTION

[0052] In order to explain the technical solution of the present invention in detail, the following will be combined with the accompanying drawings of the embodiments of the present invention to clearly and completely describe the technical solution of the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the described embodiments of the present invention, other embodiments obtained by ordinary technicians in this field without creative labor all belong to the protection scope of the present invention.

[0053] Example 1

[0054] A method for preparing a water-based conductive adhesive (reaction formula see Figure 2 , the preparation flow chart is shown in Figure 3 ), specifically comprising the following steps:

[0055] 1) Weigh 3.15g of lithium hydroxide monohydrate and dissolve it in 40g of deionized water. Slowly add 9g of acrylic acid to neutralize it in a water bath at room temperature (neutralization degree is 60%). Weigh 0.075g of azobisisobutylamidine hydrochloride and dissolve it in 10g of deionized water. Transfer the neutralized solution to a 250mL three-necked flask equipped with a condenser. Add 3g of hydroxyethyl acrylate, 3g of N-hydroxymethyl acrylamide and 40g of deionized water. Add about 5mL of initiator solution with a syringe, pass nitrogen and start mechanical stirring. After 15 minutes, start heating to 60°C. After reacting for 8h, add 3mL of initiator solution. After continuing to react for 8h, add the remaining initiator solution. After reacting for another 8h, terminate the reaction and pour out the binder solution while it is hot.

[0056] 2) Weigh 50 g of the binder solution (solid content of 14.29%), add it to 60 mL of phosphate buffer (Ph = 6.5), and stir it on a magnetic stirrer for 1 hour to disperse the binder solution. Weigh 0.4 g of carbodiimide hydrochloride and 0.3 g of N-hydroxysuccinimide and dissolve them in 20 mL of phosphate buffer. 6 g of monomer D (structural formula: Figure 1, the average value of n is 6) was dissolved in 20 mL of phosphate buffer, and the three solutions were poured into a 250 mL three-necked flask and mixed. After nitrogen was passed to exclude air, the mixture was stirred at room temperature for 9 h to obtain an aqueous conductive adhesive solution.

[0057] 3) The aqueous conductive adhesive solution was dialyzed in a 10 kDa dialysis bag, and deionized water was replaced after 8 hours of dialysis. The solution was dialyzed twice for purification to remove a small amount of unreacted monomers, thereby obtaining an aqueous conductive adhesive PAHN-PPS (solid content of 3.23%).

[0058] A method for preparing a half-cell using the aqueous conductive adhesive comprises the following steps:

[0059] 1) Weigh the silicon-carbon active material, Ketjen black and the purified aqueous conductive binder (by solid mass) in a mass ratio of 8:1:1, add deionized water according to the viscosity, grind them thoroughly in a mortar, and then apply the slurry on a copper foil with a scraper. The content of silicon-carbon active material on the copper foil is 1.46 mg cm -2 , placed in a 130℃ oven for 5h, and then placed in a 60℃ vacuum drying oven for 9h. The dried electrode was punched into a small electrode with a diameter of 10mm.

[0060] 2) Place the lithium sheet on the negative electrode shell in the glove box, add a diaphragm, drip the electrolyte, place the negative electrode sheet, gasket, and spring in sequence, then add the positive electrode shell, and finally seal it with a battery packaging machine and let it stand for 24 hours to allow the electrode to fully dissolve the electrolyte.

[0061] Figure 4 The infrared spectrum of the water-based conductive adhesive is 3500-3100 cm -1 It is a broad absorption peak formed by hydroxyl and amino groups, with a wave number of 2929cm -1 The absorption peak of methylene is at 1712 cm -1 and 1264cm -1 They are the absorption peaks of carbon group and carbon oxygen bond, indicating the existence of carboxyl group, with a wave number of 1160cm -1 It is the stretching vibration peak of carbon-nitrogen bond, indicating the presence of amide, wave number 1163cm -1 It is the absorption peak of the ether bond of long-chain fatty ether, wave number 1070cm -1 and 623cm -1 The characteristic peak of the sulfonic acid group is located at the wave number of 1680-1640cm -1 There is no absorption peak in the range, indicating that the binder does not contain carbon-carbon double bonds and the monomer reaction is relatively complete.

[0062] Figure 5a The binder has a current density of 0.325A·g -1Cyclic performance curve, the first cycle capacity is as high as 873mAh g -1 After 131 cycles, the capacity dropped to 766.52 mAh g -1 , the capacity retention rate is 87.71% and the coulombic efficiency is stable.

[0063] Figure 5b The binder has a current density of 0.65A·g -1 Cyclic performance curve, the first cycle specific capacity is 835.88 mAh g -1 After 354 cycles, the capacity dropped to 669.77 mAh g -1 The capacity retention rate is 80.13%, and the capacity drops to 589.00 mAh g after 468 cycles. -1 The capacity retention rate is 70.46%, and the coulombic efficiency is stable under this condition. From the constant current charge and discharge test of the half-cell, it can be seen that the binder has a high capacity at both low and high currents, and the battery has excellent cycle performance.

[0064] Figure 6a This is a scanning electron microscope image of the electrode prepared with the aqueous conductive binder in Example 1 before cycling. It can be seen that the electrode prepared with the silicon-carbon negative electrode has more smooth graphite sheets.

[0065] Figure 6b The scanning electron microscope image of the electrode prepared with the aqueous conductive binder in Example 1 after 100 cycles shows that a rough SEI layer has been formed on the surface. At the same time, no obvious cracks appear on the graphite sheet, indicating that the SEI layer is stable, which is one of the reasons for the excellent cycle performance of the battery.

[0066] Example 2

[0067] A water-based conductive adhesive comprises the following steps:

[0068] 1) Weigh 3.5g of lithium hydroxide monohydrate and dissolve it in 40g of deionized water. Slowly add 7.5g of acrylic acid (neutralization degree is 80%) in a water bath at room temperature for neutralization. Weigh 0.075g of azobisisobutyronitrile and dissolve it in 10g of deionized water. Transfer the neutralized solution to a 250mL three-necked flask equipped with a condenser. Add 4.5g of hydroxyethyl methacrylate, 3g of N-hydroxymethyl acrylamide and 40g of deionized water. Add about 5mL of initiator solution with a syringe, pass nitrogen and start mechanical stirring. After 15 minutes, start heating to 60°C. After reacting for 8h, add 3mL of initiator solution. After continuing to react for 8h, add the remaining initiator solution. After reacting for another 8h, terminate the reaction and pour out the binder solution while it is hot.

[0069] 2) Weigh 50 g of the binder solution (solid content of 14.41%), add it to 60 mL of phosphate buffer (Ph = 6.5), and stir it on a magnetic stirrer for 1 hour to disperse the binder solution. Weigh 0.4 g of carbodiimide hydrochloride and 0.3 g of N-hydroxysuccinimide and dissolve them in 20 mL of phosphate buffer. 6 g of monomer D (structural formula: Figure 1 , the average value of n is 6) was dissolved in 20 mL of phosphate buffer, and the three solutions were poured into a 250 mL three-necked flask and mixed. After nitrogen was passed to exclude air, the mixture was stirred at room temperature for 9 h to obtain an aqueous conductive adhesive solution.

[0070] 3) The aqueous conductive adhesive solution was dialyzed in a 10 kDa dialysis bag, and deionized water was replaced after 8 hours of dialysis. The dialysis was performed twice for purification to remove a small amount of unreacted monomers and obtain an aqueous conductive adhesive (solid content of 3.52%).

[0071] The preparation method of the half-cell of the aqueous binder is the same as that of Example 1.

[0072] Example 3

[0073] A water-based conductive adhesive comprises the following steps:

[0074] 1) Weigh 3.87g of lithium hydroxide monohydrate and dissolve it in 40g of deionized water. Slowly add 9g of itaconic acid (neutralization degree is 60%) in a water bath at room temperature for neutralization. Weigh 0.15g of azobisisobutylamidine hydrochloride and dissolve it in 10g of deionized water. Transfer the neutralized solution to a 250mL three-necked flask equipped with a condenser. Add 4.5g of hydroxyethyl acrylate, 1.5g of N-hydroxymethyl acrylamide and 50g of deionized water. Add about 5mL of initiator solution with a syringe, pass nitrogen and start mechanical stirring. After 15 minutes, start heating to 60°C. After reacting for 8h, add 3mL of initiator solution. After continuing to react for 8h, add the remaining initiator solution. After reacting for another 8h, terminate the reaction and pour out the binder solution while it is hot.

[0075] 2) Weigh 50 g of binder solution (solid content: 14.35%), add it into 60 mL of phosphate buffer (Ph=6.5), stir it on a magnetic stirrer for 1 h to disperse the binder solution, weigh 0.37 g of carbodiimide hydrochloride, 0.28 g of N-hydroxysuccinimide and dissolve them in 20 mL of phosphate buffer, and 9 g of monomer D (structural formula: Figure 1 , the average value of n is 6) was dissolved in 20 mL of phosphate buffer, and the three solutions were poured into a 250 mL three-necked flask and mixed. After nitrogen was passed to exclude air, the mixture was stirred at room temperature for 9 h to obtain an aqueous adhesive conductive agent solution.

[0076] 3) The aqueous conductive adhesive solution was dialyzed in a 10 kDa dialysis bag, and deionized water was replaced after 8 hours of dialysis. The dialysis was performed twice for purification to remove a small amount of unreacted monomers and obtain an aqueous conductive adhesive (solid content of 4.45%).

[0077] A method for preparing a half-cell using the aqueous conductive adhesive comprises the following steps:

[0078] 1) Weigh silicon-carbon active material, Ketjen black and purified water-based conductive binder (by solid mass) in a mass ratio of 90:5:5, add deionized water according to the viscosity, grind them thoroughly in a mortar, and then apply the slurry on copper foil with a scraper. The content of silicon-carbon active material on the copper foil is 1.73 mg cm -2 , placed in a 110-150℃ oven for 3-5h, and then placed in a 60℃ vacuum drying oven for 9-12h. The dried electrode is punched into a small electrode with a diameter of 10mm.

[0079] 2) Place the lithium sheet on the negative electrode shell in the glove box, add a diaphragm, drip the electrolyte, place the negative electrode sheet, gasket, and spring in sequence, then add the positive electrode shell, and finally seal it with a battery packaging machine and let it stand for 24 hours to allow the electrode to fully dissolve the electrolyte.

[0080] Example 4

[0081] A water-based binder specifically comprises the following steps:

[0082] 1) Weigh 3.5g of lithium hydroxide monohydrate and dissolve it in 40g of deionized water. Slowly add 7.5g of acrylic acid to neutralize it in a water bath at room temperature (neutralization degree is 60%). Weigh 0.075g of azobisisobutylamidine hydrochloride and dissolve it in 10g of deionized water. Transfer the neutralized solution to a 250mL three-necked flask equipped with a condenser. Add 6g of polyethylene glycol diacrylate, 1.5g of N-hydroxymethyl acrylamide and 50g of deionized water. Add about 5mL of initiator solution with a syringe, pass nitrogen and start mechanical stirring. After 15 minutes, start heating to 60°C. After reacting for 8h, add 3mL of initiator solution. After continuing the reaction for 8h, add the remaining initiator solution. After reacting for 8h, terminate the reaction and pour out the binder solution while hot.

[0083] 2) Weigh 50 g of the binder solution (solid content of 14.31%), add it to 60 mL of phosphate buffer (Ph = 6.5), and stir it on a magnetic stirrer for 1 hour to disperse the binder solution. Weigh 0.37 g of carbodiimide hydrochloride and 0.28 g of N-hydroxysuccinimide and dissolve them in 20 mL of phosphate buffer. 6 g of monomer D (structural formula: Figure 1, the average value of n is 6) was dissolved in 20 mL of phosphate buffer, and the three solutions were poured into a 250 mL three-necked flask and mixed. After nitrogen was passed to exclude air, the mixture was stirred at room temperature for 9 h to obtain an aqueous conductive adhesive solution.

[0084] 3) The aqueous conductive adhesive solution was dialyzed in a 10 kDa dialysis bag, and deionized water was replaced after 8 hours of dialysis. The solution was dialyzed twice for purification to remove a small amount of unreacted monomers and obtain an aqueous conductive adhesive (solid content of 3.13%).

[0085] The preparation method of the half-cell of the aqueous binder is the same as that of Example 3.

[0086] Comparative Example 1

[0087] A water-based binder specifically comprises the following steps:

[0088] 1) Weigh 3.15g of lithium hydroxide monohydrate and dissolve it in 40g of deionized water. Slowly add 9g of acrylic acid to neutralize it in a water bath at room temperature (neutralization degree is 60%). Weigh 0.075g of azobisisobutylamidine hydrochloride and dissolve it in 10g of deionized water. Transfer the neutralized solution to a 250mL three-necked flask equipped with a condenser. Add 3g of hydroxyethyl acrylate, 3g of N-hydroxymethyl acrylamide and 40g of deionized water. Add about 5mL of initiator solution with a syringe, pass nitrogen and start mechanical stirring. After 15 minutes, start heating to 60°C. After reacting for 8h, add 3mL of initiator solution. After continuing to react for 8h, add the remaining initiator solution. After reacting for another 8h, terminate the reaction and pour out the binder solution while it is hot.

[0089] 2) The binder solution was dialyzed in a 10 kDa dialysis bag. After 8 hours of dialysis, the deionized water was replaced. The solution was dialyzed twice for purification to remove a small amount of unreacted monomers and obtain a water-based binder (solid content of 2.89%).

[0090] The preparation method of the half-cell of the aqueous binder is the same as that of Example 1.

[0091] Comparative Example 2

[0092] A water-based binder specifically comprises the following steps:

[0093] 1) Weigh 3.15g of lithium hydroxide monohydrate and dissolve it in 40g of deionized water. Slowly add 9g of acrylic acid to neutralize it in a water bath at room temperature (neutralization degree is 60%). Weigh 0.075g of azobisisobutylamidine hydrochloride and dissolve it in 10g of deionized water. Transfer the neutralized solution to a 250mL three-necked flask equipped with a condenser. Add 40g of deionized water. Add about 5mL of initiator solution with a syringe. Pass nitrogen and start mechanical stirring. After 15 minutes, start heating to 60°C. After reacting for 8h, add 3mL of initiator solution. After continuing to react for 8h, add the remaining initiator solution. After reacting for another 8h, terminate the reaction and pour out the binder solution while it is hot.

[0094] 2) The binder solution was dialyzed in a 10 kDa dialysis bag. After 8 hours of dialysis, the deionized water was replaced. The solution was dialyzed twice for purification to remove a small amount of unreacted monomers and obtain a water-based binder (solid content of 2.78%).

[0095] The preparation method of the half-cell of the aqueous binder is the same as that of Example 1.

[0096] Comparative Example 3

[0097] Take LA133 binder and prepare half cells according to the preparation methods of Example 1 and Example 3 respectively.

[0098] Figure 5b The long-term cycle performance of three binders, PAHN-PPS of Example 1, PAHN of Comparative Example 1, and PAA of Comparative Example 2, at a current density of 0.65A / g were compared. As can be seen from the figure, the capacity and cycle performance of Comparative Example 1 are both better than those of Comparative Example 2, indicating that the network structure formed by thermal self-crosslinking is conducive to stabilizing silicon particles and reducing the impact of silicon volume expansion. The formed SEI layer is more stable, thus having a longer service life. The capacity and cycle performance of Example 1 are better than those of Comparative Example 1, indicating that the introduction of aminosulfonate containing long-chain ether bonds as side chains enhances the ion-conducting ability of the binder, reduces the resistance to the conduction of lithium ions at the negative electrode, thereby increasing the capacity of the battery, and is also more conducive to the long-term stability of the SEI layer, thereby improving the cycle performance.

[0099] Table 1 shows the viscosity, slurry ratio (ratio of active material, conductive agent and binder), slurry characteristics and 0.65A·g of the binder solution with 1% solid content of Examples 1 to 4, Comparative Example 1, Comparative Example 2 and market samples. -1 The first cycle specific capacity and the number of cycles to reach 80% of the first cycle specific capacity under the current density.

[0100] Table 1

[0101]

[0102] As can be seen from Table 1, the viscosity of the binder prepared by the present invention is higher than that of the commercially available binder. At the same time, the fluidity and adhesion of the slurry are improved to a certain extent at the same slurry ratio, and bubbles are not easily generated. The capacity and cycle performance of the battery at the same current density are also greatly improved. It can be seen that the binder provided by the present invention can be well used for silicon-based negative electrodes, enhance the conductivity of the example, reduce the influence of silicon volume expansion, form a stable SEI layer, and improve the capacity and cycle performance of the battery.

[0103] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any simple changes, substitutions, combinations, and simplifications made by any technician familiar with the profession based on the technical contents disclosed in the present invention should be regarded as equivalent replacement methods, and are included in or belong to the protection scope of the present invention.

Claims

1. A method for preparing a lithium-ion battery silicon-based negative electrode aqueous conductive binder, characterized in that: The following steps are involved: (1) dissolving lithium hydroxide in water, adding monomer A for neutralization, and the neutralization degree is 60-80%; the monomer A is at least one of acrylic acid, methacrylic acid, maleic acid, and itaconic acid; (2) mixing the neutralized solution in step (1) with monomer B, monomer C and water, adding an initiator solution to obtain a mixed solution, while passing a protective gas to remove oxygen, and then heating to 60 to 80° C. for reaction for 24 to 36 hours; the monomer B is at least one of hydroxyethyl acrylate, butyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate; and the monomer C is at least one of N-hydroxymethyl acrylamide, polyethylene glycol diacrylamide, and N-hydroxypropyl acrylamide; (3) dissolving the polymer aqueous solution obtained in step (2) in a buffer solution, adding carbodiimide hydrochloride, N-hydroxysuccinimide and monomer D, and stirring the reaction for 9 to 12 hours; the monomer D is an aminosulfonate containing a long-chain ether bond; (4) dialyzing the solution obtained in step (3) to obtain an aqueous conductive binder for a lithium-ion battery silicon-based negative electrode.

2. The preparation method according to claim 1, characterized in that: In step (1), monomer A is added in a water bath at room temperature; In step (2), the protective gas is nitrogen.

3. The preparation method according to claim 1, characterized in that: In step (2), the initiator is a combination of one or more of azobisisobutyronitrile, azobisisobutyramidine hydrochloride, ammonium persulfate, and potassium persulfate; In step (2), the mass of the initiator is 0.5-1% of the total mass of monomer A, monomer B, and monomer C; In step (2), the initiator solution is added in 3 to 4 times during the reaction.

4. The preparation method according to claim 1, characterized in that: The mass percentage content of the monomer A, monomer B, and monomer C is 40-60% of monomer A, 20-40% of monomer B, and 10-20% of monomer C, and the sum of the mass percentages of monomer A, monomer B, and monomer C is 100%; The ratio of the total mass of monomer A, monomer B, and monomer C in the mixed solution to the mass of water is (10-15): (90~85)。 5. The preparation method according to claim 1, characterized in that: In step (3), the buffer solution is a phosphate buffer solution; the pH of the buffer solution is 6.5-7; the ratio of the polymer aqueous solution to the buffer solution is 50 g: (100-150) mL; In step (3), the total mass of the carbodiimide hydrochloride and N-hydroxysuccinimide is 8-15% of the solid content in the polymer aqueous solution; the mass ratio of the carbodiimide hydrochloride and N-hydroxysuccinimide is (3-2):2; In step (3), the ratio of the molar amount of the monomer D to the molar amount of the remaining carboxyl groups after the neutralization of the monomer A is 40 to 60%; In step (3), the stirring reaction is carried out at room temperature; In step (4), the dialysis bag is a 10-15 kDa dialysis bag; and the dialysis is performed 2-3 times.

6. A lithium-ion battery silicon-based negative electrode aqueous conductive binder, characterized in that: Prepared by the preparation method according to any one of claims 1 to 5.

7. A negative electrode plate for a lithium ion battery, characterized in that: The composition comprises, by mass percentage, 80-90% of negative electrode active material, 5-10% of conductive agent, and 5-10% of aqueous binder, and the sum of the mass percentages of each component is 100%; the aqueous binder is the aqueous conductive binder for lithium-ion battery silicon-based negative electrode as described in claim 6.

8. The negative electrode plate of a lithium-ion battery according to claim 7, characterized in that: The negative electrode active material is a silicon-oxygen composite material or a silicon-carbon composite material; the conductive agent is at least one of conductive carbon black, acetylene black, graphene, conductive graphite, Ketjen black, super P, carbon nanotubes and conductive carbon fibers.

9. The negative electrode plate of a lithium-ion battery according to claim 7, characterized in that: The negative electrode active material content of the lithium ion battery negative electrode plate is 1.2 to 2.0 mg cm -2 .

10. Use of the lithium ion battery silicon-based negative electrode aqueous conductive binder according to claim 6 or the lithium ion battery negative electrode sheet according to any one of claims 7 to 9 in the preparation of lithium ion batteries.

Citation Information

Patent Citations

  • Lithium ion battery cathode binder

    CN109378478A

  • Negative electrode material, negative electrode slurry, negative electrode plate and lithium ion battery

    CN111725509A

  • Preparation method of novel multifunctional polymer binder for silicon-based negative electrode

    CN117239134A

  • Water-based polymer binder, preparation method thereof and application of water-based polymer binder in positive and negative pole pieces of lithium ion battery

    CN117363276A

  • Secondary battery negative electrode material binder and preparation method thereof