Double-layer hydrogel as well as preparation method and application thereof
The preparation of double-layer hydrogels is simplified by using spontaneous phase separation effects in one-step method, solving the problems of complex preparation and interface separation in the prior art, and achieving a tightly-bound bilayer structure and wide application prospects.
Patent Information
- Application Number
- CN202410999441.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The preparation method of existing double-layer hydrogels is complex and not universal, multi-step polymerization or requires specific raw materials, and interface separation is prone to occur, limiting its application.
By using a one-step method, the difference in the ionization ability of the first ionic monomer and the second ionic monomer in water is used to suppress the ionization degree of the second ionic monomer, reduce its solubility, and polymerize when the ionization is the same. , forming a double-layer structure.
A simplified double-layer hydrogel preparation is achieved, the two layers are tightly combined to avoid interface failure, have controllable asymmetric properties and wide application prospects, and are suitable for soft drivers and wearable devices and other fields.
Smart Images

Figure CN118930726A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogels, and in particular relates to a double-layer hydrogel and a preparation method and application thereof. Background Art
[0002] Hydrogel is one of the research hotspots in the field of soft matter, and various functions and types of hydrogels have been derived from it. Among them, double-layer hydrogels have received widespread attention due to their unique properties. Unlike traditional homogeneous system hydrogels, double-layer hydrogels have asymmetric properties on both sides, including wettability, adhesion, cross-linking density, etc. These asymmetric properties can be obtained through component adjustment or structural design, so that the two sides of the hydrogel have different functions. Due to its special asymmetric structure and the integration of multiple properties, double-layer hydrogels can achieve some functions that homogeneous hydrogels cannot achieve, and show great advantages in many fields such as tissue engineering, flexible sensing, intelligent driving, photothermal evaporation, etc.
[0003] Although there are many studies on double-layer hydrogels, there are still some problems. For example, the construction method of the double-layer structure is usually complicated, requiring multi-step polymerization or chemical modification of specific functional groups (Porous Janus materials with unique asymmetries and functionality. Linlin Yan, Xiaobin Yang, Yanqiu Zhang, Yadong Wu, Zhongjun Cheng, Seth B. Darling, Lu Shao. Materials Today, 2021, 51, 626-647), large-scale controllable preparation is difficult, and the double-layer gel may undergo interfacial separation, which greatly limits its application. One-step molding is a good means to solve the cumbersome problem of hydrogel preparation. Existing literature reports double-layer hydrogels prepared based on low critical solution temperature monomers and polymers with sol-gel transition, which are transformed from hydrophilic to hydrophobic by heating, inducing macrophase separation (Multiscale bilayer hydrogels enabled by macrophase separation. Dong Zhang, Yijing Tang, Kaihang Zhang, Yaoting Xue, Si Yu Zheng, Baoyi Wu, Jie Zheng. Matter, 2023, 6, 1484-1502), and the preparation method is simple. However, this one-step molding method requires that the two raw material components have temperature responsiveness and thermoreversible gelation, respectively, which limits the range of selectable raw materials. At present, most of the one-step preparation strategies reported also rely on specific raw material systems, and universality needs to be further improved.
[0004] Therefore, proposing a double-layer hydrogel design strategy with simple preparation process and wide applicability is of great significance for the development of functional hydrogels. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention aims to provide a double-layer hydrogel and a preparation method and application thereof.
[0006] The present invention utilizes the spontaneous phase separation effect to prepare a double-layer hydrogel by a one-step method. Specifically, the difference in ionization ability between the first ion monomer and the second ion monomer in water is utilized, and the first ion monomer is used to inhibit the degree of ionization of the second ion monomer in water, thereby reducing the solubility of the second ion monomer, thereby achieving spontaneous phase separation. At the same time, the polymerizability of the monomers is utilized so that the two electrolyte monomers can complete the polymerization reaction while phase separation, thereby achieving the effect of forming a double-layer structure.
[0007] The purpose of the present invention is achieved through the following technical solutions.
[0008] A method for preparing a double-layer hydrogel comprises the following steps:
[0009] (1) adding a first ionic monomer, a second ionic monomer, and a crosslinking agent to deionized water, and stirring until the solid is completely dissolved to obtain a mixed solution;
[0010] (2) introducing an inert gas into the mixed solution to remove dissolved oxygen, then adding a photoinitiator, stirring until the solid is completely dissolved to obtain a reaction solution, and subjecting the reaction solution to ultrasonic treatment to remove bubbles;
[0011] (3) The reaction solution is poured into a mold and allowed to stand until the reaction solution is separated into two layers and both layers of liquid are clear, and then polymerization is initiated under ultraviolet light to obtain a double-layer hydrogel.
[0012] Furthermore, in step (1), the first ionic monomer is any one of N,N,N-trimethyl-3-(2-methylacrylamide)-1-propylamine chloride, [2-(methacryloyloxy)ethyl]trimethylammonium chloride, acryloyloxyethyltrimethylammonium chloride, and (3-acrylamidopropyl)trimethylammonium chloride.
[0013] The ratio of the amount of the substance added into the first ion monomer to the volume of the deionized water is 2 mol / L to 5 mol / L.
[0014] Furthermore, in step (1), the second ionic monomer is any one of dimethylaminoethyl methacrylate, dimethylaminoethyl acrylate, 2-N-morpholineethyl methacrylate, N-[(3-(dimethylamino)propyl]methacrylamide, N-[(3-dimethylamino)propyl]acrylamide, and N-[2-(dimethylamino)ethyl]methacrylamide.
[0015] The ratio of the amount of the substance added into the second ionic monomer to the volume of the deionized water is 2 mol / L to 6 mol / L.
[0016] Furthermore, the cross-linking agent in step (1) is N,N'-methylenebispropionamide.
[0017] The amount of the cross-linking agent added is 0.1% to 0.5% of the total amount of the first ionic monomer and the second ionic monomer.
[0018] Furthermore, the inert gas in step (2) is any one of nitrogen or argon.
[0019] Furthermore, the photoinitiator in step (2) is any one of 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone or α-ketoglutaric acid.
[0020] The amount of the photoinitiator added is 0.1% to 1% of the total amount of the first ionic monomer and the second ionic monomer.
[0021] Furthermore, the power of the ultrasonic treatment in step (2) is 50W to 150W, and the ultrasonic time is 5min to 10min.
[0022] Furthermore, the mold in step (3) is any one of a transparent test tube, a polytetrafluoroethylene groove mold with a transparent cover, and a mold assembled by sandwiching a gasket between two glass plates and a long and narrow transparent sealing bag.
[0023] When using a mold assembled by two glass plates with a gasket sandwiched between them and a long and narrow transparent sealing bag, first pour the reaction liquid into the sealing bag and let it stand until the reaction liquid is separated into two layers and both layers of liquid are clear. Then, place the transparent sealing bag between the two glass plates with a gasket sandwiched between them, and slowly bring the two glass plates closer until they are clamped and sealed.
[0024] Furthermore, the wavelength of the ultraviolet light in step (3) is 320nm-365nm, the power is 80W-120W, the ultraviolet light irradiation time is 3h-12h, and the reaction temperature is 20°C-50°C.
[0025] The invention provides a double-layer hydrogel prepared by the above preparation method.
[0026] The preparation method provided by the present invention utilizes the spontaneous phase separation behavior of the system to synthesize a hydrogel with a double-layer structure through a one-step method. The upper layer and the lower layer of the gel are tightly combined with no gap between the two, and interface failure is not prone to occur.
[0027] The present invention also provides application of the double-layer hydrogel in preparing asymmetric adhesion or soft driving devices.
[0028] Compared with the prior art, the present invention has the following advantages and technical effects:
[0029] (1) The method for preparing a double-layer hydrogel provided by the present invention utilizes the spontaneous phase separation behavior of the system and obtains a layered gel through one-step polymerization. Specifically, the difference in the ionization ability of the first ion monomer and the second ion monomer in water is utilized, and the first ion monomer is used to inhibit the ionization degree of the second ion monomer in water, thereby reducing the solubility of the second ion monomer and producing an in-situ phase separation phenomenon to achieve stratification; at the same time, the polymerizability of the monomer is utilized so that the two electrolyte monomers can complete the polymerization reaction while phase separation, thereby achieving the effect of forming a double-layer structure. This method does not require complicated multi-step polymerization or surface modification, and greatly simplifies the preparation steps of the double-layer hydrogel.
[0030] (2) The double-layer hydrogel provided by the present invention has controllable asymmetric properties on both sides. The thickness, mechanical strength and adhesion of the two-layer hydrogel can be conveniently adjusted by changing the concentration of the two ionic monomers in water. In addition, since some of the optional second ionic monomers such as dimethylaminoethyl methacrylate and 2-N-morpholineethyl methacrylate are temperature-sensitive, the stratification of the system can also be controlled by changing the polymerization temperature.
[0031] (3) The double-layer hydrogel provided by the present invention exhibits asymmetric mechanical properties on both sides and is suitable for use as a soft actuator. In addition, the double-layer hydrogel with obvious asymmetric viscosity can also be used in the fields of in vivo tissue patches, wearable devices for human-machine interfaces, etc., and has broad application prospects.
[0032] (4) The preparation method of the double-layer hydrogel provided by the present invention has a certain universality, and there are many types of first ion monomers and second ion monomers that can be selected, wherein the first ion monomer is an ion monomer that can be completely ionized in water, and is a quaternary ammonium salt cationic monomer; the second ion monomer is an ion monomer with a high degree of ionization in water, and is mostly a monomer containing a tertiary amine group; these ion monomers are easy to obtain, which reduces the preparation cost. By combining different types of first ion monomers and second ion monomers, double-layer hydrogels with different properties and functions can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Scanning electron microscope and elemental energy spectrum analysis photos of the double-layer hydrogel prepared in Example 1.
[0034] Figure 2 The tensile stress-strain diagram of the upper gel and the lower gel of the double-layer hydrogel prepared in Example 1.
[0035] Figure 3 Scanning electron microscope and elemental energy spectrum analysis photos of the homogeneous hydrogel prepared in Comparative Example 1. DETAILED DESCRIPTION
[0036] The specific implementation of the present invention is further described below in conjunction with the examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art according to the prior art. If the manufacturer of the reagents or instruments used is not indicated, they are deemed to be conventional products that can be purchased commercially.
[0037] The present invention is further described below in conjunction with the examples. The hydrogel obtained in the examples was measured for tensile strength, elongation at break and adhesive strength using the method disclosed in J. Mater. Chem. C, 2023, 11, 2316-2327. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0038] The stirring described in the following examples was all carried out at room temperature.
[0039] Example 1
[0040] At room temperature, 3.5 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-chloropropylamine and 4 mol dimethylaminoethyl methacrylate were added to 1 L of deionized water and stirred for 10 min. Then, 0.023 mol N,N'-methylenebispropionamide was added and stirred until the solid was completely dissolved. Then, nitrogen was introduced to remove oxygen in the mixed solution. Finally, 0.015 mol 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added and stirred until the solid was completely dissolved to obtain a reaction solution. The reaction solution was ultrasonicated for 5 min to remove bubbles in the reaction solution. Pour the reaction liquid into a long and narrow transparent sealed bag and let it stand for 0.5 h to allow the reaction liquid to separate into two layers and both layers of liquid are clear. Then place the transparent sealed bag between two glass plates sandwiched with a gasket, and slowly bring the two glass plates closer until they are clamped and sealed. Finally, place the mold under an 80 W ultraviolet lamp with a wavelength of 320 nm for 3 h to initiate polymerization. The reaction temperature is 20°C to obtain a double-layer hydrogel.
[0041] Figure 1 The scanning electron microscope and elemental energy spectrum analysis images of the double-layer hydrogel prepared in Example 1. Figure 1 It can be seen that the hydrogel has a double-layer structure, and the upper and lower layers of the gel are tightly bound, with no gap between them, indicating that the two layers of the double-layer hydrogel constructed using the spontaneous phase separation effect are tightly bound. There is also an obvious difference in chlorine elements between the two layers, with very little chlorine elements in the upper layer and more chlorine elements in the lower layer, indicating that the upper layer of the gel is mainly formed by the polymerization of dimethylaminoethyl methacrylate monomers, and the lower layer of the gel is mainly formed by the polymerization of N,N,N-trimethyl-3-(2-methylallylamino)-1-propylamine chloride monomers.
[0042] Figure 2 The tensile stress-strain diagram of the upper and lower layers of the double-layer hydrogel prepared in Example 1. Figure 1 It can be seen that the tensile strength of the upper layer of the double-layer hydrogel prepared in Example 1 is 1200 kPa, and the elongation at break is 300%; the tensile strength of the lower layer of the gel is 80 kPa, and the elongation at break is 450%, indicating that the double-layer hydrogel has asymmetric mechanical properties and is suitable for use as a soft actuator.
[0043] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 1 is about 1:5, the upper layer is hard and non-sticky, with a tensile strength of 1200 kPa, an elongation at break of 300%, and an adhesion strength of 5 kPa; the lower layer is soft and sticky, with a tensile strength of 80 kPa, an elongation at break of 450%, and an adhesion strength of 40 kPa. The double-layer hydrogel exhibits obvious asymmetric viscosity and has potential application prospects in the fields of in vivo tissue patches, wearable devices for human-machine interfaces, and the like.
[0044] Example 2
[0045] At room temperature, 5 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-chloropropylamine and 2 mol dimethylaminoethyl methacrylate were added to 1L of deionized water, stirred for 10 minutes, and then 0.007 mol N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, and then nitrogen was introduced to remove oxygen in the mixed solution. Finally, 0.007 mol 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a long and narrow transparent sealed bag, and allowed to stand for 0.5 hours so that the reaction solution was divided into two layers and both layers of liquid were clear. Then the transparent sealed bag was placed between two glass plates sandwiched with a gasket, and the two glass plates were slowly brought close to each other until they were clamped and sealed. Finally, the mold was placed under an ultraviolet lamp with a power of 80W and a wavelength of 320nm for 3 hours to initiate polymerization. The reaction temperature was 20°C to obtain a double-layer hydrogel.
[0046] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 2 is about 1:10, the upper layer is hard and non-sticky, with a tensile strength of 1000 kPa, an elongation at break of 400%, and an adhesive strength of 5 kPa; the lower layer is soft and sticky, with a tensile strength of 100 kPa, an elongation at break of 500%, and an adhesive strength of 60 kPa.
[0047] Example 3
[0048] At room temperature, 2 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-chloropropylamine and 6 mol dimethylaminoethyl methacrylate were added to 1L of deionized water, stirred for 10 minutes, and then 0.040 mol N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, and then nitrogen was introduced to remove oxygen in the mixed solution, and finally 0.024 mol 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a long and narrow transparent sealed bag, and allowed to stand for 0.5 hours so that the reaction solution was divided into two layers and both layers of liquid were clear. Then the transparent sealed bag was placed between two glass plates sandwiched with a gasket, and the two glass plates were slowly brought close to each other until they were clamped and sealed. Finally, the mold was placed under an ultraviolet lamp with a power of 80W and a wavelength of 320nm for 4 hours to initiate polymerization. The reaction temperature was 20°C to obtain a double-layer hydrogel.
[0049] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 3 is about 1:2. The upper layer is hard and non-sticky, with a tensile strength of 1400 kPa, an elongation at break of 200%, and an adhesive strength of 5 kPa; the lower layer is soft and weakly sticky, with a tensile strength of 60 kPa, an elongation at break of 300%, and an adhesive strength of 10 kPa.
[0050] Example 4
[0051] At room temperature, 5 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-chloropropylamine and 2 mol dimethylaminoethyl acrylate were added to 1L of deionized water, stirred for 10 minutes, and then 0.007 mol N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, and then nitrogen was introduced to remove oxygen in the mixed solution. Finally, 0.035 mol 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a long and narrow transparent sealed bag, and allowed to stand for 0.5 hours so that the reaction solution was divided into two layers and both layers of liquid were clear. Then, the transparent sealed bag was placed between two glass plates sandwiched with a gasket, and the two glass plates were slowly brought close to each other until they were clamped and sealed. Finally, the mold was placed under an ultraviolet lamp with a power of 80W and a wavelength of 320nm for 4 hours to initiate polymerization. The reaction temperature was 20°C to obtain a double-layer hydrogel.
[0052] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 4 is about 1:10, the upper layer is hard and non-sticky, with a tensile strength of 800 kPa, an elongation at break of 400%, and an adhesive strength of 5 kPa; the lower layer is soft and sticky, with a tensile strength of 100 kPa, an elongation at break of 500%, and an adhesive strength of 60 kPa.
[0053] Example 5
[0054] At room temperature, 2 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-chloropropylamine and 6 mol dimethylaminoethyl acrylate were added to 1L of deionized water, stirred for 10 minutes, and then 0.040 mol N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, and then nitrogen was introduced to remove oxygen in the mixed solution. Finally, 0.056 mol 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a long and narrow transparent sealed bag, and allowed to stand for 1 hour so that the reaction solution was divided into two layers and both layers of liquid were clear. Then the transparent sealed bag was placed between two glass plates sandwiched with a gasket, and the two glass plates were slowly brought close to each other until they were clamped and sealed. Finally, the mold was placed under an ultraviolet lamp with a power of 80W and a wavelength of 320nm for 5 hours to initiate polymerization. The reaction temperature was 20°C to obtain a double-layer hydrogel.
[0055] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 5 is about 1:2. The upper layer is hard and non-sticky, with a tensile strength of 1000 kPa, an elongation at break of 200%, and an adhesive strength of 5 kPa; the lower layer is soft and weakly sticky, with a tensile strength of 60 kPa, an elongation at break of 300%, and an adhesive strength of 10 kPa.
[0056] Example 6
[0057] At room temperature, 5 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-propylamine chloride and 2 mol 2-N-morpholineethyl methacrylate were added to 1L deionized water, stirred for 10 minutes, and then 0.007 mol N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, and then nitrogen was introduced to remove oxygen in the mixed solution, and finally 0.063 mol 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a polytetrafluoroethylene groove mold, and allowed to stand for 1 hour so that the reaction solution was divided into two layers and both layers of liquid were clear, and then a transparent cover was covered, and finally the mold was placed under a 100W ultraviolet lamp with a wavelength of 320nm for 5 hours to initiate polymerization, and the reaction temperature was 20°C to obtain a double-layer hydrogel.
[0058] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 6 is about 1:10, the upper layer is hard and non-sticky, with a tensile strength of 1100 kPa, an elongation at break of 400%, and an adhesive strength of 5 kPa; the lower layer is soft and sticky, with a tensile strength of 100 kPa, an elongation at break of 500%, and an adhesive strength of 60 kPa.
[0059] Example 7
[0060] At room temperature, 2 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-chloropropylamine and 6 mol 2-N-morpholineethyl methacrylate were added to 1L deionized water, stirred for 10 minutes, and then 0.040 mol N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, and then nitrogen was introduced to remove oxygen in the mixed solution, and finally 0.080 mol 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a polytetrafluoroethylene groove mold, and allowed to stand for 1 hour so that the reaction solution was divided into two layers and both layers of liquid were clear, and then a transparent cover was covered, and finally the mold was placed under a 100W ultraviolet lamp with a wavelength of 320nm for 6 hours to initiate polymerization, and the reaction temperature was 20°C to obtain a double-layer hydrogel.
[0061] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 7 is about 1:2. The upper layer is hard and non-sticky, with a tensile strength of 1500 kPa, an elongation at break of 200%, and an adhesive strength of 5 kPa; the lower layer is soft and weakly sticky, with a tensile strength of 60 kPa, an elongation at break of 300%, and an adhesive strength of 10 kPa.
[0062] Example 8
[0063] At room temperature, 5 mol [2-(methacryloyloxy)ethyl]trimethylammonium chloride and 2 mol N-[(3-(dimethylamino)propyl]methacrylamide were added to 1L of deionized water and stirred for 10 minutes. Then, 0.007 mol N,N'-methylenebispropionamide was added and stirred until the solid was completely dissolved. Then, argon was introduced to remove oxygen from the mixed solution. Finally, 0.007 mol α-ketoglutaric acid was added and stirred until the solid was completely dissolved to obtain a reaction solution. The reaction solution was ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a polytetrafluoroethylene groove mold and allowed to stand for 1.5 hours so that the reaction solution was divided into two layers and both layers of liquid were clear. Then, a transparent cover was placed on the mold. Finally, the mold was placed under a 100 W ultraviolet lamp with a wavelength of 365 nm for 6 hours to initiate polymerization. The reaction temperature was 35°C to obtain a double-layer hydrogel.
[0064] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 8 is about 1:30. The upper layer is hard and non-sticky, with a tensile strength of 900 kPa, an elongation at break of 400%, and an adhesive strength of 5 kPa; the lower layer is soft and sticky, with a tensile strength of 120 kPa, an elongation at break of 500%, and an adhesive strength of 60 kPa.
[0065] Example 9
[0066] At room temperature, 2 mol [2-(methacryloyloxy)ethyl]trimethylammonium chloride and 6 mol N-[(3-(dimethylamino)propyl]methacrylamide were added to 1 L of deionized water and stirred for 10 min. Then, 0.040 mol N,N'-methylenebispropionamide was added and stirred until the solid was completely dissolved. Then, argon was introduced to remove oxygen from the mixed solution. Finally, 0.016 mol α-ketoglutaric acid was added and stirred until the solid was completely dissolved to obtain a reaction solution. The reaction solution was ultrasonicated for 5 min to remove bubbles in the reaction solution. The reaction solution was poured into a polytetrafluoroethylene groove mold and allowed to stand for 1.5 h to allow the reaction solution to separate into two layers and both layers of liquid to be clear. Then, a transparent cover was placed on the mold. Finally, the mold was placed under a 100 W UV lamp with a wavelength of 365 nm for 7 h to initiate polymerization. The reaction temperature was 35 ° C to obtain a double-layer hydrogel.
[0067] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 9 is about 1:3. The upper layer is hard and non-sticky, with a tensile strength of 1300 kPa, an elongation at break of 200%, and an adhesive strength of 5 kPa; the lower layer is soft and weakly sticky, with a tensile strength of 80 kPa, an elongation at break of 300%, and an adhesive strength of 10 kPa.
[0068] Example 10
[0069] At room temperature, 5 mol of acryloyloxyethyl trimethylammonium chloride and 2 mol of N-[(3-dimethylamino)propyl] acrylamide were added to 1L of deionized water, stirred for 10 minutes, and then 0.007 mol of N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, and then argon was introduced to remove oxygen in the mixed solution, and finally 0.021 mol of α-ketoglutaric acid was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a polytetrafluoroethylene groove mold, and allowed to stand for 1.5 hours so that the reaction solution was divided into two layers and both layers of liquid were clear, and then a transparent cover was placed on it, and finally the mold was placed under a 100W ultraviolet lamp with a wavelength of 365nm for 8 hours to initiate polymerization, and the reaction temperature was 35°C to obtain a double-layer hydrogel.
[0070] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 10 is about 1:10, the upper layer is hard and non-sticky, with a tensile strength of 700 kPa, an elongation at break of 400%, and an adhesive strength of 5 kPa; the lower layer is soft and non-sticky, with a tensile strength of 110 kPa, an elongation at break of 500%, and an adhesive strength of 5 kPa.
[0071] Embodiment 11
[0072] At room temperature, 2 mol of acryloyloxyethyl trimethylammonium chloride and 6 mol of N-[(3-dimethylamino)propyl] acrylamide were added to 1L of deionized water, stirred for 10 minutes, and then 0.040 mol of N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, then argon was introduced to remove oxygen in the mixed solution, and finally 0.040 mol of α-ketoglutaric acid was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a transparent test tube, and allowed to stand for 1.5 hours so that the reaction solution was divided into two layers and both layers of liquid were clear, and then the tube mouth was sealed with a sealing film, and finally the mold was placed under a 120W ultraviolet lamp with a wavelength of 365nm for 9 hours to initiate polymerization, and the reaction temperature was 35°C to obtain a double-layer hydrogel.
[0073] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 11 is about 1:2, the upper layer is hard and non-sticky, with a tensile strength of 1100 kPa, an elongation at break of 200%, and an adhesive strength of 5 kPa; the lower layer is soft and non-sticky, with a tensile strength of 70 kPa, an elongation at break of 300%, and an adhesive strength of 5 kPa.
[0074] Example 12
[0075] At room temperature, 5 mol (3-acrylamidopropyl) trimethylammonium chloride and 2 mol N-[2-(dimethylamino)ethyl] methacrylamide were added to 1L deionized water, stirred for 10 minutes, and then 0.007 mol N, N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, then argon was introduced to remove oxygen in the mixed solution, and finally 0.049 mol α-ketoglutaric acid was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a transparent test tube, and allowed to stand for 1.5 hours so that the reaction solution was divided into two layers and both layers of liquid were clear, and then the tube mouth was sealed with a sealing film, and finally the mold was placed under a 120W ultraviolet lamp with a wavelength of 365nm for 10 hours to initiate polymerization, and the reaction temperature was 35°C to obtain a double-layer hydrogel.
[0076] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 12 is about 1:10. The upper layer is hard and non-sticky, with a tensile strength of 800 kPa, an elongation at break of 400%, and an adhesive strength of 5 kPa; the lower layer is soft and sticky, with a tensile strength of 90 kPa, an elongation at break of 500%, and an adhesive strength of 60 kPa.
[0077] Embodiment 13
[0078] At room temperature, 2 mol (3-acrylamidopropyl) trimethylammonium chloride and 6 mol N-[2-(dimethylamino)ethyl] methacrylamide were added to 1L deionized water, stirred for 10 minutes, and then 0.040 mol N, N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, then argon was introduced to remove oxygen in the mixed solution, and finally 0.072 mol α-ketoglutaric acid was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a transparent test tube, and allowed to stand for 2 hours so that the reaction solution was divided into two layers and both layers of liquid were clear, and then the tube mouth was sealed with a sealing film, and finally the mold was placed under a 120W ultraviolet lamp with a wavelength of 365nm for 11 hours to initiate polymerization, and the reaction temperature was 35°C to obtain a double-layer hydrogel.
[0079] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 13 is approximately 1:2. The upper layer is hard and non-sticky, with a tensile strength of 1200 kPa, an elongation at break of 200%, and an adhesive strength of 5 kPa; the lower layer is soft and weakly sticky, with a tensile strength of 50 kPa, an elongation at break of 300%, and an adhesive strength of 10 kPa.
[0080] Embodiment 14
[0081] At room temperature, 5 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-chloropropylamine and 2 mol dimethylaminoethyl methacrylate were added to 1L of deionized water, stirred for 10 minutes, and then 0.007 mol N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, and then nitrogen was introduced to remove oxygen in the mixed solution. Finally, 0.007 mol 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a long and narrow transparent sealed bag, and allowed to stand for 0.5 hours so that the reaction solution was divided into two layers and both layers of liquid were clear. Then, the transparent sealed bag was placed between two glass plates sandwiched with a gasket, and the two glass plates were slowly brought close to each other until they were clamped and sealed. Finally, the mold was placed under an ultraviolet lamp with a power of 80W and a wavelength of 320nm for 3 hours to initiate polymerization. The reaction temperature was 50°C to obtain a double-layer hydrogel.
[0082] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 14 is about 1:7, the upper layer is hard and non-sticky, with a tensile strength of 1100 kPa, an elongation at break of 400%, and an adhesive strength of 5 kPa; the lower layer is soft and sticky, with a tensile strength of 90 kPa, an elongation at break of 500%, and an adhesive strength of 60 kPa.
[0083] Embodiment 15
[0084] At room temperature, 5 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-chloropropylamine and 2 mol 2-N-morpholineethyl methacrylate were added to 1L deionized water, stirred for 10 minutes, and then 0.007 mol N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, and then nitrogen was introduced to remove oxygen in the mixed solution, and finally 0.063 mol 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a polytetrafluoroethylene groove mold, and allowed to stand for 1 hour so that the reaction solution was divided into two layers and both layers of liquid were clear, and then a transparent cover was covered, and finally the mold was placed under a 100W ultraviolet lamp with a wavelength of 320nm for 5 hours to initiate polymerization, and the reaction temperature was 50°C to obtain a double-layer hydrogel.
[0085] The volume stratification ratio of the upper and lower layers of the double-layer hydrogel prepared in Example 15 is about 1:7. The upper layer is hard and non-sticky, with a tensile strength of 1200 kPa, an elongation at break of 400%, and an adhesive strength of 5 kPa; the lower layer is soft and sticky, with a tensile strength of 90 kPa, an elongation at break of 500%, and an adhesive strength of 60 kPa.
[0086] By comparing Example 2 and Example 14, and Example 6 and Example 15, it can be seen that by only changing the polymerization temperature, the double-layer hydrogels obtained in Example 2 and Example 14 or Example 4 and Example 15 have different stratification ratios. This is because the second ion monomers dimethylaminoethyl methacrylate and 2-N-morpholineethyl methacrylate are temperature-sensitive, and the stratification of the system can be controlled by temperature.
[0087] Comparative Example 1
[0088] At room temperature, 1 mol N,N,N-trimethyl-3-(2-methylallylamino)-1-chloropropylamine and 1 mol dimethylaminoethyl methacrylate were added to 1L of deionized water, stirred for 10 minutes, and then 0.002 mol N,N'-methylenebispropionamide was added, stirred until the solid was completely dissolved, then argon was introduced to remove oxygen in the mixed solution, and finally 0.020 mol α-ketoglutaric acid was added, stirred until the solid was completely dissolved to obtain a reaction solution, and ultrasonicated for 5 minutes to remove bubbles in the reaction solution. The reaction solution was poured into a transparent test tube, and allowed to stand for 2 hours so that the reaction solution was divided into two layers and both layers of liquid were clear, and then the tube mouth was sealed with a sealing film, and finally the mold was placed under a 120W ultraviolet lamp with a wavelength of 365nm for 12 hours to initiate polymerization, and the reaction temperature was 50°C to obtain a hydrogel.
[0089] The hydrogel prepared in Comparative Example 1 is a homogeneous system without stratification. Figure 3 The scanning electron microscope and elemental energy spectrum analysis photos of the homogeneous hydrogel prepared in Comparative Example 1 are shown in FIG. Figure 3 It can be seen that the carbon, oxygen and chlorine elements are evenly distributed in the hydrogel, and there is no difference in element distribution, which means that layered hydrogel cannot be prepared at this formula concentration.
[0090] It can be seen from Comparative Example 1 that when the amount of the first ionic monomer N,N,N-trimethyl-3-(2-methylallylamino)-1-propylamine chloride and the second ionic monomer dimethylaminoethyl methacrylate added is small, that is, when the concentration of the first ionic monomer or the second ionic monomer in water does not reach the concentration range described in the present invention, phase separation will not occur in the system, and a hydrogel with a double-layer structure cannot be prepared.
Claims
1. A method for preparing a double-layer hydrogel, It is characterized in that The steps include: (1) adding a first ionic monomer, a second ionic monomer, and a crosslinking agent to deionized water, and stirring until the solid is completely dissolved to obtain a mixed solution; (2) introducing an inert gas into the mixed solution, then adding a photoinitiator, stirring until the solid is completely dissolved to obtain a reaction solution, and subjecting the reaction solution to ultrasonic treatment; (3) The reaction solution is poured into a mold and allowed to stand until the reaction solution is separated into two layers and both layers of liquid are clear, and then polymerization is initiated under ultraviolet light to obtain a double-layer hydrogel.
2. A method for preparing a double-layer hydrogel according to claim 1, It is characterized in that Step (1) The first ionic monomer is any one of N,N,N-trimethyl-3-(2-methylacrylamide)-1-propylamine chloride, [2-(methacryloyloxy)ethyl]trimethylammonium chloride, acryloxyethyltrimethylammonium chloride, and (3-acrylamidepropyl)trimethylammonium chloride; the ratio of the amount of the first ionic monomer added to the volume of deionized water is 2 mol / L to 5 mol / L.
3. The method for preparing a double-layer hydrogel according to claim 1, It is characterized in that Step (1) The second ionic monomer is any one of dimethylaminoethyl methacrylate, dimethylaminoethyl acrylate, 2-N-morpholineethyl methacrylate, N-[(3-(dimethylamino)propyl]methacrylamide, N-[(3-dimethylamino)propyl]acrylamide, and N-[2-(dimethylamino)ethyl]methacrylamide; the ratio of the amount of the second ionic monomer added to the volume of deionized water is 2 mol / L to 6 mol / L.
4. The method for preparing a double-layer hydrogel according to claim 1, It is characterized in that The cross-linking agent in step (1) is N,N'-methylenebispropionamide; the amount of the cross-linking agent added is 0.1% to 0.5% of the total amount of the first ionic monomer and the second ionic monomer.
5. The method for preparing a double-layer hydrogel according to claim 1, It is characterized in that The photoinitiator in step (2) is any one of 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone and α-ketoglutaric acid; the amount of the photoinitiator added is 0.1% to 1% of the total amount of the first ionic monomer and the second ionic monomer.
6. The method for preparing a double-layer hydrogel according to claim 1, It is characterized in that The inert gas in step (2) is any one of nitrogen or argon.
7. The method for preparing a double-layer hydrogel according to claim 1, It is characterized in that The mold in step (3) is any one of a transparent test tube, a polytetrafluoroethylene groove mold with a transparent cover, and a mold assembled by sandwiching a gasket between two glass plates and a long and narrow transparent sealing bag.
8. The method for preparing a double-layer hydrogel according to claim 1, It is characterized in that The wavelength of the ultraviolet light in step (3) is 320nm-365nm, the power is 80W-120W, the ultraviolet light irradiation time is 3h-12h, and the reaction temperature is 20°C-50°C.
9. A double-layer hydrogel prepared by the preparation method according to any one of claims 1 to 8, It is characterized in that It has the property of being asymmetrical on both sides.
10. Use of the double-layer hydrogel according to claim 9 in preparing asymmetric adhesion or soft driving devices.
Citation Information
Patent Citations
Preparation method, product and application of double-layer water gel with salt-temperature dual response
CN108395548A
Method for preparing asymmetric-structure hydrogel in one step by means of difference in viscosity, product of method and application of product
CN110229286A
Thermosensitive single-layer hydrogel with controllable transparency, preparation method and assembled double-layer hydrogel
CN114891241A
Preparation method of multi-structure anisotropic hydrogel based on oxygen-heat dual drive
CN116284864A
Multifunctional hydrogel with microphase separation structure as well as preparation method and application of multifunctional hydrogel
CN117164890A