High-grafting-rate soluble polyethylene grafted maleic anhydride material prepared with assistance of nitrogen-containing organic matter and preparation method of high-grafting-rate soluble polyethylene grafted maleic anhydride material

By using nitrogen-containing organics and suitable initiators in the preparation of polyethylene grafted maleic anhydride materials, combined with high-speed mixing and extrusion processes, the grafting rate and processing performance problems caused by side reactions in traditional processes are solved, and the problem of grafting rate and processing performance is achieved. High grafting rate and excellent processing performance significantly improve the toughening and capacity enhancement effect of the material.

CN118930741APending Publication Date: 2024-11-12SHANDONG JIANBANG NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411163780.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional polyethylene grafted maleic anhydride materials are prone to side reactions when prepared at high temperatures, resulting in a decrease in graft rate, poor processing performance, and the odor of styrene affects product quality.

Method used

The high-graft rate soluble polyethylene graft maleic anhydride material is assisted by nitrogen-containing organic matter. The extrusion temperature and screw speed are controlled through the combination of high-speed mixer and twin-screw extruder, and stearamide and N-A are used. Nitrogen-containing organic substances such as acetamide and DCP/BPO initiators inhibit side reactions and improve grafting rate and processing performance.

Benefits of technology

It effectively inhibits the side reaction of polyethylene grafted maleic anhydride material, improves the grafting rate and processing performance, significantly improves its toughening and capacity enhancement effects, and improves the regularity and application performance of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-grafting-rate soluble polyethylene grafted maleic anhydride material prepared with assistance of a nitrogen-containing organic matter and a preparation method of the high-grafting-rate soluble polyethylene grafted maleic anhydride material. The preparation method comprises the following steps: S1, sufficiently and uniformly mixing polyethylene, MAH, an initiator, the nitrogen-containing organic matter, paraffin oil and an antioxidant 168 according to a certain mass ratio by using a high-speed mixer, and then standing for a period of time; and S2, carrying out melt grafting on the mixture through a twin-screw extruder, reasonably setting the temperatures of different temperature zones of the extruder, carrying out water-cooling pelletizing on the extruded material, and carrying out drying treatment to obtain the soluble polyethylene grafted MAH material with the high grafting rate. The product prepared by the invention has high grafting rate and excellent processability when being used as a compatilizer, and the compatibilization and toughening effects of the compatilizer can be remarkably improved by a more regular macromolecular chain structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional polymer materials, and in particular to a nitrogen-containing organic matter-assisted high-grafting rate soluble polyethylene grafted maleic anhydride material and a preparation method thereof. Background Art

[0002] Functionalized polyolefins are widely used in the fields of polymer material modification and composite material preparation. Among them, various types of polyethylene grafted with maleic anhydride have a wide hardness range and operating temperature, and can be used as a toughening agent and compatibilizer for polar plastics or organic-inorganic composite materials. Its toughening mechanism is mainly the silver-crack-shear band theory, and the system mainly forms a "sea-island" structure.

[0003] The melt grafting process generally involves fully blending polyolefin, grafting monomer, initiator and comonomer in advance, and then adding them to the screw extruder for melt grafting reaction. In the plasticizing extrusion system, high temperature melts the polymer, reduces its viscosity and forms a fluid. Therefore, melt grafting uses the crossflow of the molten fluid in the screw to achieve the purpose of further fully mixing the polymer and the grafting monomer. However, the higher preparation temperature will accelerate the decomposition of the initiator to produce free radicals, causing the polymer and the monomer to undergo a rapid grafting reaction. Since the temperature required for melt grafting of polyolefin is relatively high, the initiator quickly decomposes in a short time to produce primary free radicals, which then capture the hydrogen atoms on the polyolefin molecules to produce a large number of polyolefin macromolecular free radicals. The polyolefin macromolecular free radicals cannot be grafted with the monomer in time, and are prone to side reactions such as β-fracture and cross-linking branching. Moreover, the development of side reactions is different for different macromolecular structures. The above problems will lead to monomer residues, changes in physical properties and decreased processing performance, which will affect the grafting rate and the quality of the functionalized polyolefin. In addition, the second monomer is usually styrene, and its own odor will also affect the quality of the final product. For polyethylene materials, cross-linking side reactions are the main trend. When PE melt is mixed with initiator free radicals at high temperature, branched cross-linking points are easily formed. The probability of the above cross-linking reaction occurring in the presence of MAH increases sharply. Therefore, the processing performance of PE-g-MAH prepared under traditional processes is significantly reduced compared with PE, which seriously affects its application performance. Therefore, a nitrogen-containing organic matter-assisted preparation of a high grafting rate soluble polyethylene grafted maleic anhydride material and a preparation method thereof are proposed to solve the above problems. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes a nitrogen-containing organic matter-assisted preparation of a high grafting rate soluble polyethylene grafted maleic anhydride material and a preparation method thereof. In order to achieve the above technical objectives and the above technical effects, the present invention is implemented by the following technical solutions: The present invention proposes a nitrogen-containing organic compound-assisted preparation of a high grafting rate soluble polyethylene grafted maleic anhydride material, comprising the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168, wherein the mass ratio of polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168 is 100: 1.5-1.8: 0.3-0.4: 0.1-0.5: 0.2: 0.3.

[0005] In a preferred embodiment, the preparation method comprises the following steps: S1: Use a high-speed mixer to fully mix polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168 according to a certain mass ratio and leave it for a period of time; S2: The mixture is melt-grafted through a twin-screw extruder, and the temperature of different temperature zones of the extruder is reasonably set. The extruded material is water-cooled and pelletized, and then dried to obtain a soluble polyethylene-grafted MAH material with a high grafting rate.

[0006] In a preferred embodiment, in step S2, the extrusion temperatures of each temperature zone of the extruder are set to 80°C, 100°C, 160°C, 190°C, 200°C, 200°C, 205°C, 210°C and 200°C, respectively, and the screw speed of the extruder is set to 200-300r / min.

[0007] In a preferred embodiment, the nitrogen-containing organic matter includes one of stearamide, N-methylacetamide, N,N-dimethylacetamide, N,N-diethyl-m-toluamide, caprolactam, N-methylpyrrolidone, N,N-dimethylaniline, and 2,6-lutidine-N-oxide.

[0008] In a preferred embodiment, the initiator is DCP and BPO in a ratio of 2:1-3:1.

[0009] Beneficial effects of the present invention: 1) The present invention proposes a nitrogen-containing organic compound-assisted preparation of a high grafting rate soluble polyethylene grafted maleic anhydride material and a preparation method thereof. Compounds with electron-donating effects, such as a large number of nitrogen-containing organic compounds, can inhibit the homopolymerization of MAH through electron transfer reactions. This effect can effectively inhibit the coupling reaction between different grafted chains during the PE grafting MAH process, and at the same time obtain a PE-g-MAH grafted material with a more uniform structure; 2) The present invention proposes a nitrogen-containing organic matter-assisted preparation of a high-grafting rate soluble polyethylene grafted maleic anhydride material and a preparation method thereof. The prepared product has a high grafting rate and excellent processing performance when used as a compatibilizer, and the more regular macromolecular chain structure can significantly improve its volume-increasing and toughening effects. DETAILED DESCRIPTION

[0010] The present invention will be further explained below in conjunction with specific embodiments. Example 1

[0011] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, stearamide, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100: 1.5: 0.4: 0.2: 0.1: 0.2: 0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Example 2

[0012] This embodiment proposes a method of preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, N-methylacetamide, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100:1.5:0.4:0.2:0.1:0.2:0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Example 3

[0013] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, N,N-diethyl-m-toluamide, paraffin oil and antioxidant 168 are uniformly mixed in a high-speed mixer at a mass ratio of 100: 1.5: 0.4: 0.2: 0.1: 0.2: 0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Example 4

[0014] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, N,N-diethyl-m-toluamide, paraffin oil and antioxidant 168 are uniformly mixed in a high-speed mixer at a mass ratio of 100: 1.6: 0.4: 0.2: 0.1: 0.2: 0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Example 5

[0015] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, caprolactam, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100: 1.5: 0.4: 0.2: 0.1: 0.2: 0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Example 6

[0016] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, N-methylpyrrolidone, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100:1.5:0.4:0.2:0.1:0.2:0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Example 7

[0017] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; PE, MAH, initiator, N,N-dimethylaniline, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100:1.5:0.4:0.2:0.1:0.2:0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Example 8

[0018] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, 2,6-lutidine-N-oxide, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100: 1.5: 0.4: 0.2: 0.1: 0.2: 0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Example 9

[0019] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, N,N-diethyl-m-toluamide, paraffin oil and antioxidant 168 are uniformly mixed in a high-speed mixer at a mass ratio of 100: 1.8: 0.4: 0.2: 0.1: 0.2: 0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Example 10

[0020] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, N,N-diethyl-m-toluamide, paraffin oil and antioxidant 168 are uniformly mixed in a high-speed mixer at a mass ratio of 100: 1.8: 0.4: 0.5: 0.1: 0.2: 0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate. Embodiment 11

[0021] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, N,N-dimethylaniline, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100:1.8:0.4:0.2:0.1:0.2:0.3; The temperature of each zone of the twin-screw extruder was set to 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C. The screw speed was 300 r / min, and the mixed raw materials were added. The extruded materials were water-cooled and pelletized, and then dried to obtain a soluble polyethylene grafted MAH material with a high grafting rate. Example 12

[0022] This embodiment proposes a method for preparing a high grafting rate soluble polyethylene grafted maleic anhydride material with the aid of nitrogen-containing organic matter, which includes the following raw materials: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168; Polyethylene, MAH, initiator, N,N-dimethylaniline, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100:1.8:0.4:0.5:0.1:0.2:0.3; The temperatures of each zone of the twin-screw extruder were set at 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C, the screw speed was 300 r / min, the mixed raw materials were added, the extruded materials were water-cooled and pelletized, and then dried to obtain soluble polyethylene-grafted MAH materials with high grafting rate.

[0023] Among them, the initiator in Example 1-12 is a mixture of DCP and BPO in a ratio of 3:1.

[0024] Comparative Example 1 Polyethylene, MAH, DCP, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100: 1.5: 0.4: 0.2: 0.3; The temperature of each zone of the twin-screw extruder was set to 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C. The screw speed was 300 r / min, and the mixed raw materials were added. The extruded materials were water-cooled and pelletized, and then dried to obtain a soluble polyethylene grafted MAH material with a high grafting rate.

[0025] Comparative Example 2 Polyethylene, MAH, DCP, paraffin oil and antioxidant 168 were uniformly mixed in a high-speed mixer at a mass ratio of 100: 1.8: 0.4: 0.2: 0.3; The temperature of each zone of the twin-screw extruder was set to 80, 100, 160, 190, 200, 200, 205, 210 and 200 °C. The screw speed was 300 r / min, and the mixed raw materials were added. The extruded materials were water-cooled and pelletized, and then dried to obtain a soluble polyethylene grafted MAH material with a high grafting rate.

[0026] Performance Testing Purification of PE-g-MAH: Weigh 10g of the grafted product and put it into 200ml of xylene solution, heat and reflux, and filter out insoluble impurities after the grafted product is fully dissolved. Pour it into acetone solution while hot to obtain a white flocculent precipitate, filter it and vacuum dry it to obtain purified PE-g-MAH.

[0027] 1. Determination of grafting rate Weigh about 0.5g of the purified grafted product, add 200ml of toluene, heat and stir for 1h, cool to room temperature, add 30ml (0.05M) potassium hydroxide ethanol solution, heat and reflux for 2h, then add phenolphthalein as an indicator, and back titrate with (0.05M) hydrogen chloride isopropanol solution. Then calculate the grafting rate by the following formula.

[0028] , V is the volume of the solution, C is the molar concentration of the solution, is the mass of PE-g-MAH, and 98.06 is the molecular weight of MAH.

[0029] 2. Melt index determination The melt index of the sample is tested according to GB / T 3682-2000 at 190°C and a load of 2.16kg. The test time interval is 30s. The test sample is a granular material. The sample is measured in parallel 5 times and the average value is taken.

[0030] Table 1 PE-g-MAH grafting rate and melt index Grafting rate / % Melt index / (g / 10min) Comparative Example 1 0.89 2.44 Comparative Example 2 0.82 1.23 Example 1 0.97 3.32 Example 2 0.98 3.37 Example 3 1.08 3.52 Example 4 1.12 3.48 Example 5 1.04 3.55 Example 6 1.05 3.67 Example 7 1.22 3.34 Example 8 0.88 3.68 Example 9 1.16 3.56 Example 10 1.28 3.43 Embodiment 11 1.30 3.36 Example 12 1.38 3.42 The PE is Mobil 3518CB and the melt index is 3.5 g / 10min.

[0031] From the above data, we can see that: (1) Under the traditional formula of comparative example 1-2, PE crosslinking is more obvious during the grafting process, and the melt index decreases from 3.5 g / 10 min to 2.44 g / 10 min. At the same time, increasing the amount of MAH and initiator does not increase the grafting rate, but further promotes the crosslinking reaction, and the melt index further decreases to 1.23 g / 10 min, and the grafting rate is less than 0.9%.

[0032] (2) It can be seen from Examples 1-8 that, under the same formula ratio, the formula containing N,N-diethyl-m-toluamide and N,N-dimethylaniline has a higher grafting rate and maintains good processing performance.

[0033] (3) From Examples 9-12, it can be seen that increasing the ratio of MAH and nitrogen-containing organic matter is beneficial to improving the grafting rate, and the processing performance does not change much.

[0034] (4) From Examples 1-12 and Control Examples 1-2, it can be seen that the initiation effect of the DCP / BPO composite initiator is better than that of the single DCP initiator. This is because the addition of BPO is beneficial to the electron transfer reaction in the early stage of the grafting reaction, avoiding the occurrence of cross-linking reaction and increasing the grafting rate of MAH.

[0035] The PE-g-MAH and PA6 prepared in Example 12 and Comparative Example 2 were extruded and granulated in a twin-screw at a mass ratio of 85 / 15, and finally injection molded into standard specimens for mechanical property testing, wherein the PA6 brand was Ube 1030b.

[0036] Table 2 Mechanical properties of PA6 / PE-g-MAH blends performance PA6 Comparative Example 2 Example 12 Tensile Strength 63.3 MPa 52.5 MPa 58.4 MPa Notched impact strength <![CDATA[7.1kJ / m 2 ]]> <![CDATA[9.7kJ / m 2 ]]> <![CDATA[25.6kJ / m 2 ]]> Bending Strength 104.5 MPa 44.2Mpa 64.7MPa Taking PE / glass fiber mass ratio of 65 / 30 as the basic system, 5 parts of PE-g-MAH prepared in Example 12 and Comparative Example 2 were added and mixed, extruded into granules in a twin-screw, and finally injection molded into standard specimens for mechanical property testing. Among them, the PE brand is Mobil 3518CB.

[0037] Table 3 Mechanical properties of PE / glass fiber / PE-g-MAH composites performance Comparative Example 2 Example 12 Tensile Strength 47.3 MPa 88.8 MPa Notched impact strength <![CDATA[6.1kJ / m 2 ]]> <![CDATA[16.7kJ / m 2 ]]> Bending Strength 56.2 MPa 78.3Mpa From the application performance test, it can be seen that the PE-g-MAH prepared in Example 12 has a better toughening effect on PA6, and the volume-increasing effect on the PE / glass fiber system is significantly better than that of Comparative Example 12. This is because the PE-g-MAH prepared in Example 12 has a higher grafting rate and better processing performance, is more evenly distributed in the system, and has a smaller dispersed size.

[0038] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A nitrogen-containing organic compound-assisted preparation of a high grafting rate soluble polyethylene grafted maleic anhydride material, characterized in that: Including the following ingredients: Polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168, wherein the mass ratio of polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168 is 100: 1.5-1.8: 0.3-0.4: 0.1-0.5: 0.2: 0.

3.

2. The method of preparing a high grafting rate soluble polyethylene grafted maleic anhydride material assisted by nitrogen-containing organic matter according to claim 1, characterized in that: The preparation method thereof comprises the following steps: S1: Use a high-speed mixer to fully mix polyethylene, MAH, initiator, nitrogen-containing organic matter, paraffin oil and antioxidant 168 according to a certain mass ratio and leave it for a period of time; S2: The mixture is melt-grafted through a twin-screw extruder, and the temperature of different temperature zones of the extruder is reasonably set. The extruded material is water-cooled and pelletized, and then dried to obtain a soluble polyethylene-grafted MAH material with a high grafting rate.

3. The method of preparing a high grafting rate soluble polyethylene grafted maleic anhydride material assisted by nitrogen-containing organic matter according to claim 2, characterized in that: In step S2, the extrusion temperatures of each temperature zone of the extruder are set to 80°C, 100°C, 160°C, 190°C, 200°C, 200°C, 205°C, 210°C and 200°C, respectively, and the screw speed of the extruder is set to 200-300r / min.

4. The method of preparing a high grafting rate soluble polyethylene grafted maleic anhydride material assisted by nitrogen-containing organic matter according to claim 1, characterized in that: The nitrogen-containing organic matter includes one of stearamide, N-methylacetamide, N,N-dimethylacetamide, N,N-diethyl-m-toluamide, caprolactam, N-methylpyrrolidone, N,N-dimethylaniline, and 2,6-dimethylpyridine-N-oxide.

5. The method of preparing a high grafting rate soluble polyethylene grafted maleic anhydride material assisted by nitrogen-containing organic matter according to claim 1, characterized in that: The initiator is DCP and BPO in a ratio of 2:1-3:1.