Ultrahigh-temperature-resistant ceramic resin as well as preparation method and application thereof
Through the combination of modified polyimide resin and composite ceramic filler, the problem of poor thermal stability of ceramic resin at high temperatures is solved, its mechanical properties and high temperature resistance are improved, and it is suitable for photocuring 3D printing, meeting aerospace and other Material requirements in the field.
Patent Information
- Application Number
- CN202411350391.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing ceramic resins have poor thermal stability and insufficient mechanical strength at high temperatures, making them difficult to meet the demand for high temperature, wear and corrosion-resistant materials in the aerospace, military industry and other fields.
Modified polyimide resin, modified alumina and silica as composite ceramic fillers, the aromatic spirocyclic compounds and amide acids are synthesized, and fluorine atoms and amino groups are introduced to increase the thermodynamic stability and solubility of the molecules. The specific surface area and dispersion of alumina are improved by acidification treatment, and the cross-linking network density is increased by combining with the active diluent.
It has achieved the improvement of ultra-high temperature resistance and mechanical properties of ceramic resin, improved its reliability and market value at high temperatures, and is suitable for photocuring 3D printing.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic resins, and in particular relates to an ultra-high temperature resistant ceramic resin and a preparation method and application thereof. Background Art
[0002] Photocuring technology is a process that uses light energy to initiate the curing of materials. It has the advantages of fast curing speed, low energy consumption, and environmental friendliness. In the preparation of ceramic resin, the addition of photoinitiator enables the resin to cure quickly under light of a specific wavelength, providing an efficient and controllable curing method for 3D printing. With the continuous improvement of material performance requirements in aerospace, military industry, and energy development, the demand for high temperature resistant, wear resistant, and corrosion resistant materials is growing. Ceramic resin is a material composed of an inorganic ceramic material and an organic resin matrix. The excellent performance of ceramic fillers and photosensitive resins combined with the convenience of photocuring technology provide a new material choice for 3D printing technology.
[0003] Photosensitive resin is the core material of photocurable 3D printing technology, which directly affects the quality and characteristics of the printed products. Common photosensitive resins on the market mainly include epoxy resin, acrylic resin and polyester resin. However, the products printed by these resins generally have problems such as insufficient mechanical strength, large shrinkage and poor thermal stability. Due to its unique molecular structure, photosensitive polyimide resin exhibits excellent heat resistance and excellent mechanical and chemical properties. It is also photosensitivity. The photo-crosslinkable active groups contained in its molecules can induce chemical reactions under ultraviolet light to form a three-dimensional cross-linked network structure, which improves the mechanical strength, thermal stability and chemical stability of the material after curing, thereby greatly expanding the application range of polyimide materials.
[0004] Chinese patent CN 110357592 A discloses a ceramic resin for 3D printing, which is composed of nano-ceramic filler and photocurable resin; wherein the nano-ceramic filler is composed of the following substances: topological carbon nanostructure filler, silicon dioxide, aluminum oxide; the photocurable resin is composed of the following substances: epoxy acrylic resin, active diluent, photoinitiator, inert diluent butyl acetate, the ceramic resin provided by this invention can effectively improve the mechanical properties of ceramic shell membrane materials, thereby reducing the breakage rate of the shell membrane and improving the yield rate of cast products. However, the photocurable resin is epoxy acrylic resin, which has poor thermal stability.
[0005] Therefore, there is an urgent need for an ultra-high temperature resistant ceramic resin and a preparation method and application thereof, so that it can withstand ultra-high temperatures and have good mechanical properties. Summary of the invention
[0006] In view of the existing technical problems, the purpose of the present invention is to provide a ceramic resin resistant to ultrahigh temperature and its preparation method and application. The ceramic resin of the present invention has ultrahigh temperature resistance and good mechanical properties, can be used for photocuring 3D printing, and has good market value.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] The present invention first provides an ultra-high temperature resistant ceramic resin, which comprises the following raw materials by weight: 30-50 parts of modified polyimide resin, 40-60 parts of composite ceramic filler, 20-35 parts of active diluent, and 2-5 parts of photoinitiator.
[0009] The reaction mechanism and effects of the present invention are as follows:
[0010] 1. The main chain of aromatic polyimide contains a large number of aromatic rings and imide rings, and has excellent properties such as high rigidity, high melting point, good heat resistance, good chemical resistance, high mechanical strength, and radiation resistance. However, due to the rigidity of the main chain structure, the high symmetry of the molecular structure, and the strong interaction between molecular chains, it may show crystallinity and make the polyimide molecular chains densely stacked, resulting in traditional polyimide being difficult to melt or dissolve, making it difficult to process.
[0011] Aromatic spiro compounds have a special spiro cross-rigid structure. A series of polymers synthesized from them have a high melting point and glass transition temperature, which can improve the thermodynamic stability of molecules, inhibit the crystallization of molecules, and improve the solubility and stability of materials.
[0012] The present application adopts acetaminophen and 2,7-dihydroxy-9-fluorenone to synthesize an aromatic spiro compound, thereby improving the solubility. Then, the applicant reduces the amide group to an amino group, introduces hexafluorodianhydride and γ-aminopropyltriethoxysilane, and caps it with phthalic anhydride to form a precursor of modified polyimide, polyamic acid; finally, the double bond is grafted by reacting the hydroxyl group on the synthesized compound 2 with the epoxy group, so that the polyimide has a photosensitive group.
[0013] On the one hand, hexafluorodianhydride contains fluorine atoms, which, combined with the benzene ring structure, can enhance the van der Waals force between molecules, especially the high electronegativity of fluorine atoms, which can enhance the dipole-dipole interaction between molecules; at the same time, the CF bond formed by fluorine atoms and carbon atoms is very stable and difficult to break at high temperatures, and the introduction of hexafluorobenzoic anhydride increases the number of aromatic rings. The introduction of fluorine atoms and the rigidity of aromatic rings can improve the thermal stability of the polymer;
[0014] On the other hand, γ-aminopropyltriethoxysilane contains amino groups, which increase the polarity of the polymer. The amino groups can also form hydrogen bonds with solvent molecules, which helps to improve the solubility of the polymer in the solvent. In addition, the introduction of triethoxysilane groups can increase the flexibility of the polymer chain, reduce entanglement between chains, and make the polymer easier to dissolve.
[0015] 2. Add modified alumina and silica as composite ceramic fillers to high temperature resistant ceramic resin. Alumina provides high strength and high temperature resistance, while silica provides good chemical stability and wear resistance. By controlling the particle size and ratio of the two, the applicant can better improve the hardness, strength and wear resistance of the ceramic resin, thereby enhancing its mechanical properties; it can also effectively adjust the thermal expansion coefficient of the ceramic resin and reduce thermal stress, thereby improving the reliability of the material under temperature changes and improving high temperature resistance.
[0016] In order to improve the mechanical strength, the proportion of alumina in the system may often be increased, but the increase in the alumina content will affect the curing performance of the resin, leaving more defects in the product during photocuring. For modified alumina, the present invention increases the specific surface area and porosity of alumina by acidifying the alumina, and the subsequent modification steps are to improve the dispersibility and compatibility of alumina with other materials, thereby greatly increasing the solid phase content when alumina and resin are mixed without affecting the photocuring effect, further improving the mechanical properties.
[0017] 3. The active diluent used in the present invention increases the density of the cross-linked network, prevents the generation of cracks to a certain extent, has a toughening and strengthening effect, and can improve the mechanical properties of the photocurable polyimide resin.
[0018] In some embodiments, the method for preparing the modified polyimide resin comprises the following steps:
[0019] S1. Add acetaminophen and 2,7-dihydroxy-9-fluorenone into a reaction kettle, add p-toluenesulfonic acid under an inert gas atmosphere, and heat to 130-150°C for 2-3h;
[0020] S2. After the system is cooled to 70-80°C, methanol is added and stirred for 0.5-1h to obtain a solution, which is poured into deionized water to produce a precipitate, which is filtered and washed. The filter cake obtained by filtration is dissolved in ethyl acetate to obtain a solution, which is then extracted with ethyl acetate for 3-4 times. The organic phase is collected, distilled under reduced pressure, and purified by silica gel column chromatography to obtain compound 1;
[0021] S3. Compound 1 obtained in step S2 and concentrated hydrochloric acid were mixed, heated to 70-75° C., stirred for 8-14 h, filtered, and washed 3-4 times to obtain compound 2;
[0022] S4. Add compound 2 obtained in step S3, hexafluorodianhydride, γ-aminopropyltriethoxysilane and N-methylpyrrolidone to a reactor, stir at 0-2°C for 4-5h, add phthalic anhydride and stir for 50-70min, heat to 55-65°C and react for 100-130min, then heat to 100-120°C and react for 100-130min, finally heat to 180-210°C and react for 3.5-4.5h, cool to 30-35°C, then add triethylamine, tetraethylammonium bromide, glycidyl methacrylate and hydroquinone, heat to 95-105°C and stir for 3-4h, cool to room temperature, pour into deionized water for precipitation, filter, wash and dry to obtain a modified polyimide resin.
[0023] In some embodiments, the molar ratio of acetaminophen to 2,7-dihydroxy-9-fluorenone in step S1 is (2.05-2.6):1.
[0024] In some embodiments, the molar ratio of compound 2, hexafluorodianhydride, γ-aminopropyltriethoxysilane and phthalic anhydride in step S4 is 6:(6-8):(6-8):(1-3).
[0025] In some embodiments, the eluent for the silica gel column chromatography purification in step S2 is dichloromethane:methanol=80:1 (V / V).
[0026] In some embodiments, the concentration of the concentrated hydrochloric acid in step S3 is 11-12 mol / L, and the molar ratio of compound 1 to concentrated hydrochloric acid is 1:(2-4).
[0027] In some embodiments, the composite ceramic filler is modified alumina with a particle size of 10-12 μm and silicon dioxide with a particle size of 2-4 μm, and the mass ratio of the two is (30-40):1.
[0028] In some embodiments, the method for preparing the modified alumina comprises the following steps:
[0029] (1) mixing aluminum oxide, concentrated nitric acid and concentrated sulfuric acid, reflux reacting in an oil bath at 100-120° C. for 1-1.5 hours, filtering, washing and drying to obtain activated aluminum oxide;
[0030] (2) Dispersing the activated alumina obtained in step (1) in anhydrous ethanol, adding a surfactant, heating to 70-80°C and stirring for 2-3h, then dropping a polymer hyperdispersant, reflux reacting at 85-95°C for 4-5h, drying, crushing and sieving to obtain modified alumina.
[0031] In some embodiments, the mass ratio of the aluminum oxide, the surfactant and the polymer hyperdispersant in step (2) is 100:(1-5):(0.8-4).
[0032] In some embodiments, the mass ratio of aluminum oxide to anhydrous ethanol in step (2) is 1:(8-12).
[0033] In some embodiments, the surfactant in step (2) is fatty alcohol polyoxyethylene ether.
[0034] In some embodiments, the polymer hyperdispersant in step (2) is an acrylic block copolymer and / or an organosilicon dispersant.
[0035] Preferably, the polymer hyperdispersant in step (2) is an acrylic block copolymer and an organosilicon dispersant, and the mass ratio of the two is 3:1.
[0036] In some embodiments, the reactive diluent is at least two of N-vinyl pyrrolidone, lauryl methacrylate, and polyethylene glycol diacrylate.
[0037] Preferably, the active diluent is N-vinyl pyrrolidone, lauryl methacrylate and polyethylene glycol diacrylate, and the mass ratio of the three is 3:1:1.
[0038] In some embodiments, the photoinitiator is any one of TPO, TPO-L and 819.
[0039] The present invention also provides a method for preparing an ultrahigh temperature resistant ceramic resin, comprising the following steps:
[0040] The modified polyimide resin and the composite ceramic filler are added into a reaction kettle, stirred and mixed, and then an active diluent and a photoinitiator are added, stirred and mixed, and vacuum degassing is performed to obtain a ceramic resin resistant to ultrahigh temperature.
[0041] The third aspect of the present invention provides an application of ultra-high temperature resistant ceramic resin for photocuring 3D printing.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] 1. The ceramic resin of the present invention has ultra-high temperature resistance and good mechanical properties, can be used for photocuring 3D printing, and has good market value.
[0044] 2. The modified polyimide of the present invention has a photosensitive group after modification, which improves the solubility and thermal stability.
[0045] 3. The modified alumina of the present invention has good dispersibility and compatibility. By further controlling the particle size and ratio of the modified alumina and silica, the hardness, strength, wear resistance and high temperature resistance of the ceramic resin can be better improved.
[0046] 4. The active diluent of the present invention increases the density of the cross-linked network and improves the mechanical properties of the photocurable polyimide resin. DETAILED DESCRIPTION
[0047] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, rather than to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0048] According to the ratios of the raw materials and the preparation methods specified in the following examples and comparative examples, various ultrahigh temperature resistant resins were prepared.
[0049] In order to facilitate those skilled in the art to implement the present invention, some raw material manufacturers of the embodiments and comparative examples are described as follows:
[0050] Polyethylene glycol diacrylate: purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., molecular weight 400;
[0051] Fatty alcohol polyoxyethylene ether AEO-3: purchased from Shandong Yunxin New Material Technology Co., Ltd.;
[0052] Acrylic block copolymer Efka PX 4300: purchased from Shanghai Ruifu Chemical Co., Ltd.;
[0053] Organic silicon dispersant PSI-500: purchased from Shanghai Yinghe Chemical Technology Co., Ltd.;
[0054] Silicon dioxide: purchased from Weifang Sanjia Chemical Co., Ltd., particle size 3 μm and 10 μm;
[0055] Alumina: purchased from Henan Taoang Industrial Co., Ltd., particle size 12 μm;
[0056] Other raw materials are not specially specified and can be purchased from the market.
[0057] Preparation Example 1
[0058] The preparation method of modified polyimide resin A comprises the following steps:
[0059] S1. Add 22 mmol of acetaminophen and 10 mmol of 2,7-dihydroxy-9-fluorenone into a reaction kettle, add 16 mmol of p-toluenesulfonic acid under an inert gas atmosphere, and heat to 140°C for 2.5 hours;
[0060] S2. After the system is cooled to 75°C, 10 ml of methanol is added and stirred for 0.5 h. The obtained solution is poured into 100 ml of deionized water to produce a precipitate. The precipitate is filtered and washed three times with deionized water. The filter cake obtained by filtration is dissolved in 100 ml of ethyl acetate. After obtaining a solution, it is extracted three times with ethyl acetate. The organic phase is collected and distilled under reduced pressure. Compound 1 is purified by silica gel column chromatography. The eluent for purification is dichloromethane:methanol=80:1 (V / V);
[0061] S3. 8 mmol of compound 1 obtained in step S2 and 16 mmol of 12 mol / L concentrated hydrochloric acid were mixed, heated to 70° C., stirred for 10 h, filtered, and washed 4 times with deionized water to obtain compound 2;
[0062] S4. Add 6mmol of compound 2, 7mmol of hexafluorodianhydride, 7mmol of γ-aminopropyltriethoxysilane and 25ml of N-methylpyrrolidone obtained in step S3 to a reactor, stir at 0°C for 4h, add 2mol of phthalic anhydride and stir for another 1h, heat to 60°C for reaction for 2h, then heat to 105°C for reaction for 2h, finally heat to 195°C for reaction for 4h, cool to 35°C, then add 16mg of triethylamine, 36mg of tetraethylammonium bromide, 6.6mmol of glycidyl methacrylate and 48mg of hydroquinone, heat to 100°C for stirring for 3h, cool to room temperature, pour the solution into 100ml of distilled water for precipitation, filter, wash 3 times with deionized water, and dry at 40°C for 18h to obtain modified polyimide resin A.
[0063] Preparation Example 2
[0064] The preparation method of modified polyimide resin B is the same as that of Preparation Example 1, except that in step S1, 19.2 mmol of acetaminophen and 12.8 mmol of 2,7-dihydroxy-9-fluorenone are added to a reaction kettle, 16 mmol of p-toluenesulfonic acid is added under an inert gas atmosphere, and the mixture is heated to 140° C. and reacted for 2.5 hours.
[0065] Preparation Example 3
[0066] The preparation method of modified polyimide resin C is the same as that of Preparation Example 1, except that the amount of hexafluorodianhydride added in step S4 is 5 mmol.
[0067] Preparation Example 4
[0068] The preparation method of modified polyimide resin D is the same as that of Preparation Example 1, except that the amount of γ-aminopropyltriethoxysilane added in step S4 is 5 mmol.
[0069] Preparation Example 5
[0070] The preparation method of modified aluminum oxide A comprises the following steps:
[0071] (1) 20 g of aluminum oxide, 0.5 L of 68 wt% concentrated nitric acid and 1.5 L of 98 wt% concentrated sulfuric acid were mixed, refluxed in an oil bath at 100° C. for 1 h, filtered, washed with deionized water until neutral, and dried at 105° C. for 3 h to obtain activated aluminum oxide;
[0072] (2) Disperse 15 g of the activated alumina obtained in step (1) in 150 ml of anhydrous ethanol, add 0.45 g of fatty alcohol polyoxyethylene ether AEO-3, heat to 75° C. and stir for 2.5 h, then dropwise add 0.225 g of acrylic block copolymer Efka PX 4300 and 0.15 g of silicone dispersant PSI-500, control the dropping time to 30 min, reflux at 85° C. for 4.5 h, dry at 100° C. for 6 h, crush and sieve to obtain modified alumina A with a particle size of 12 μm.
[0073] Preparation Example 6
[0074] The preparation method of modified alumina B is the same as that of Preparation Example 5, except that the amount of fatty alcohol polyoxyethylene ether AEO-3 added in step (2) is 0.9 g.
[0075] Preparation Example 7
[0076] The preparation method of modified alumina C is the same as that of Preparation Example 5, except that the amount of acrylic block copolymer Efka PX 4300 added in step (2) is 0.045 g and the amount of organosilicon dispersant PSI-500 is 0.03 g.
[0077] Example 1
[0078] A ceramic resin resistant to ultrahigh temperatures comprises the following raw materials, measured by weight: 40 parts of modified polyimide resin A, 48.5 parts of modified alumina A, 1.4 parts of silicon dioxide with a particle size of 3 μm, 16.5 parts of N-vinyl pyrrolidone, 5.5 parts of lauryl methacrylate, 5.5 parts of polyethylene glycol diacrylate, and 8193.5 parts of a photoinitiator.
[0079] The preparation method of the ceramic resin of this embodiment comprises the following steps:
[0080] Add modified polyimide resin A, modified alumina A, and silicon dioxide into a reactor, stir for 3 hours to mix, then add N-vinyl pyrrolidone, lauryl methacrylate, polyethylene glycol diacrylate, and photoinitiator 819, stir for 2 hours to mix, and vacuum degassing to obtain an ultra-high temperature resistant ceramic resin.
[0081] Example 2
[0082] A ceramic resin resistant to ultrahigh temperatures comprises the following raw materials, measured by weight: 30 parts of modified polyimide resin A, 38.75 parts of modified aluminum oxide A, 1.25 parts of silicon dioxide with a particle size of 3 μm, 12 parts of N-vinyl pyrrolidone, 4 parts of lauryl methacrylate, 4 parts of polyethylene glycol diacrylate, and 8192 parts of a photoinitiator.
[0083] The preparation method of the ceramic resin in this embodiment is the same as that in Example 1.
[0084] Example 3
[0085] A ceramic resin resistant to ultrahigh temperatures comprises the following raw materials, measured by weight: 50 parts of modified polyimide resin A, 58.5 parts of modified aluminum oxide A, 1.5 parts of silicon dioxide with a particle size of 3 μm, 25 parts of N-vinyl pyrrolidone, 10 parts of polyethylene glycol diacrylate, and 8195 parts of a photoinitiator.
[0086] The preparation method of the ceramic resin in this embodiment is the same as that in Example 1.
[0087] Example 4
[0088] A ceramic resin resistant to ultrahigh temperature and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified polyimide resin B is used to replace modified polyimide resin A.
[0089] Example 5
[0090] A ceramic resin resistant to ultrahigh temperature and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified polyimide resin C is used to replace modified polyimide resin A.
[0091] Example 6
[0092] A ceramic resin resistant to ultrahigh temperature and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified polyimide resin D is used to replace modified polyimide resin A.
[0093] Example 7
[0094] A ceramic resin resistant to ultrahigh temperatures and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified alumina B is used to replace modified alumina A.
[0095] Example 8
[0096] A ceramic resin resistant to ultrahigh temperatures and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified alumina C is used to replace modified alumina A.
[0097] Example 9
[0098] A ceramic resin resistant to ultrahigh temperatures and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that 27.5 parts of N-vinyl pyrrolidone are used to replace 16.5 parts of N-vinyl pyrrolidone, 5.5 parts of lauryl methacrylate and 5.5 parts of polyethylene glycol diacrylate.
[0099] Example 10
[0100] A ceramic resin resistant to ultrahigh temperatures and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of silicon dioxide with a particle size of 10 μm is used to replace silicon dioxide with a particle size of 3 μm.
[0101] Comparative Example 1
[0102] A ceramic resin resistant to ultrahigh temperatures and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of commercially available alumina with a particle size of 12 μm is used to replace modified alumina A.
[0103] Effect evaluation:
[0104] The ceramic resins prepared in the above Examples 1-10 and Comparative Example 1 were tested and analyzed, and the specific results are shown in Table 1.
[0105] Performance Test:
[0106] The ceramic resin was subjected to light curing test, and the heat deformation temperature referred to the standard GB / T 1634.2-2019; the tensile strength referred to the standard GB / T1040-1992.
[0107] Table 1
[0108] Serial number Heat deformation temperature / ℃ Tensile strength / MPa Example 1 489 122 Example 2 462 110 Example 3 476 116 Example 4 340 106 Example 5 394 119 Example 6 407 112 Example 7 379 99 Example 8 355 95 Example 9 426 103 Example 10 406 108 Comparative Example 1 338 89
[0109] From the results in Table 1, it can be seen that the ceramic resins prepared in Examples 1-3 have high temperature resistance and good mechanical properties, and have good market value.
[0110] Compared with Example 1, the molar ratio of acetaminophen and 2,7-dihydroxy-9-fluorenone was changed when preparing the modified polyimide resin in Example 4, so that it could not better synthesize aromatic spiro compounds, affecting the high temperature resistance and mechanical properties of the synthesized modified polyimide resin.
[0111] Compared with Example 1, in Example 5-6, the molar ratio of hexafluorodianhydride, γ-aminopropyltriethoxysilane, phthalic anhydride and compound 2 was changed when preparing the modified polyimide resin, which reduced the solubility and thermal stability of the resin, thereby affecting the high temperature resistance and mechanical properties of the ceramic resin.
[0112] Compared with Example 1, Examples 7-8 changed the mass ratio of surfactant, polymer hyperdispersant and alumina when preparing modified alumina, which reduced the dispersibility and compatibility of the modified alumina, thereby affecting the high temperature resistance and mechanical properties of the ceramic resin.
[0113] Compared with Example 1, Example 9 uses only one active diluent, N-vinyl pyrrolidone, which reduces the cross-linking network density, thereby reducing the high temperature resistance and mechanical properties of the ceramic resin.
[0114] Compared with Example 1, Example 10 uses an equal amount of silica with a particle size of 10 μm to replace silica with a particle size of 3 μm, which weakens the synergy of the composite ceramic filler, affects the thermal expansion coefficient of the ceramic resin, and further leads to a decrease in tensile strength.
[0115] Compared with Example 1, Comparative Example 1 uses commercially available alumina with a particle size of 12 μm to replace modified alumina A. The above is only a preferred embodiment of the present invention, and does not limit the present application in any form. Although the present application is disclosed as above in the preferred embodiment, it is not used to limit the present application. Any technician familiar with this profession, without departing from the scope of the technical solution of the present application, makes slight changes or modifications using the technical content disclosed above, which are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.
Claims
1. A ceramic resin resistant to ultra-high temperatures, It is characterized in that The invention comprises the following raw materials by weight: 30-50 parts of modified polyimide resin, 40-60 parts of composite ceramic filler, 20-35 parts of active diluent and 2-5 parts of photoinitiator.
2. The ultrahigh temperature resistant ceramic resin according to claim 1, It is characterized in that The preparation method of the modified polyimide resin comprises the following steps: S1. Add acetaminophen and 2,7-dihydroxy-9-fluorenone into a reaction kettle, add p-toluenesulfonic acid under an inert gas atmosphere, and heat to 130-150°C for 2-3h; S2. After the system is cooled to 70-80°C, methanol is added and stirred for 0.5-1h to obtain a solution, which is poured into deionized water to produce a precipitate, which is filtered and washed. The filter cake obtained by filtration is dissolved in ethyl acetate to obtain a solution, which is then extracted with ethyl acetate for 3-4 times. The organic phase is collected, distilled under reduced pressure, and purified by silica gel column chromatography to obtain compound 1; S3. Compound 1 obtained in step S2 and concentrated hydrochloric acid were mixed, heated to 70-75° C., stirred for 8-14 h, filtered, and washed 3-4 times to obtain compound 2; S4. Add compound 2 obtained in step S3, hexafluorodianhydride, γ-aminopropyltriethoxysilane and N-methylpyrrolidone to a reactor, stir at 0-2°C for 4-5h, add phthalic anhydride and stir for 50-70min, heat to 55-65°C and react for 100-130min, then heat to 100-120°C and react for 100-130min, finally heat to 180-210°C and react for 3.5-4.5h, cool to 30-35°C, then add triethylamine, tetraethylammonium bromide, glycidyl methacrylate and hydroquinone, heat to 95-105°C and stir for 3-4h, cool to room temperature, pour into deionized water for precipitation, filter, wash and dry to obtain a modified polyimide resin.
3. The ultrahigh temperature resistant ceramic resin according to claim 2, It is characterized in that The molar ratio of acetaminophen to 2,7-dihydroxy-9-fluorenone in step S1 is (2.05-2.6):
1.
4. The ultrahigh temperature resistant ceramic resin according to claim 2, It is characterized in that The molar ratio of compound 2, hexafluorodianhydride, γ-aminopropyltriethoxysilane and phthalic anhydride in step S4 is 6:(6-8):(6-8):(1-3).
5. The ultrahigh temperature resistant ceramic resin according to claim 1, It is characterized in that The composite ceramic filler is modified alumina with a particle size of 10-12 μm and silicon dioxide with a particle size of 2-4 μm, and the mass ratio of the two is (30-40):
1.
6. The ultrahigh temperature resistant ceramic resin according to claim 5, It is characterized in that The preparation method of the modified alumina comprises the following steps: (1) mixing aluminum oxide, concentrated nitric acid and concentrated sulfuric acid, reflux reacting in an oil bath at 100-120° C. for 1-1.5 hours, filtering, washing and drying to obtain activated aluminum oxide; (2) Dispersing the activated alumina obtained in step (1) in anhydrous ethanol, adding a surfactant, heating to 70-80°C and stirring for 2-3h, then dropping a polymer hyperdispersant, reflux reacting at 85-95°C for 4-5h, drying, crushing and sieving to obtain modified alumina.
7. The ultrahigh temperature resistant ceramic resin according to claim 6, It is characterized in that The mass ratio of the aluminum oxide, the surfactant and the polymer hyperdispersant in step (2) is 100:(1-5):(0.8-4).
8. The ultrahigh temperature resistant ceramic resin according to claim 1, It is characterized in that The active diluent is at least two of N-vinyl pyrrolidone, lauryl methacrylate and polyethylene glycol diacrylate.
9. A method for preparing the ultrahigh temperature resistant ceramic resin according to any one of claims 1 to 8, It is characterized in that The following steps are included: The modified polyimide resin and the composite ceramic filler are added into a reaction kettle, stirred and mixed, and then an active diluent and a photoinitiator are added, stirred and mixed, and vacuum degassing is performed to obtain a ceramic resin resistant to ultrahigh temperature.
10. An application of the ultrahigh temperature resistant ceramic resin according to any one of claims 1 to 8, It is characterized in that For light-curing 3D printing.