High-temperature-resistant insulating resin material

By combining bisphenol F and nanofillers, a stronger epoxy resin material is formed, which solves the problem of poor insulation performance and harmful gas release at high temperatures, and achieves higher high temperature resistance and insulation performance , improves the safety and environmental performance of electrical equipment.

CN118930813APending Publication Date: 2024-11-12ZHEJIANG ZHONGDA CABLE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411216766.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing high-temperature resistant epoxy resin materials are prone to release harmful gases or substances at high temperatures, which can cause harm to human health and the environment, and there is room for optimization of insulation performance, resulting in insufficient safety in the power field.

Method used

Bisphenol F is used as the base material, and by combining it with nanofillers (such as nanosilicon, nanozirconia and nanoalumina), and using phenolic resin as a curing agent, the cross-linking density and flame retardant properties of epoxy resin are increased to form a more Strong and stable three-dimensional mesh structure to avoid degradation of insulation performance and release of harmful gases at high temperatures.

Benefits of technology

It significantly improves the insulation performance and high temperature resistance of epoxy resin, avoids the degradation of insulation performance and release of harmful gases at high temperatures, reduces the risk of electrical equipment failure, and improves the flame retardant performance of the material and the safety of the human body environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930813A_ABST
    Figure CN118930813A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant insulating resin material, and relates to the technical field of resin material preparation, and a preparation method of the resin material comprises the following steps: S1, raw material preparation; s2, synthesizing bisphenol F type epoxy resin; s3, modification treatment; and S4, carrying out post-treatment. According to the high-temperature-resistant insulating resin material, bisphenol F is taken as a base material, and a proper curing agent is added, so that the crosslinking density of epoxy resin is increased, and the epoxy resin is firmer and more stable, so that the insulating property of the epoxy resin is remarkably improved, and the prepared insulating resin material has excellent high-temperature-resistant performance and can be used as a high-temperature-resistant material in a high-temperature environment; the insulation structure of the electrical equipment can be effectively prevented from losing efficacy, risks of electrical faults such as electric leakage and short circuit are reduced, in addition, harmful gas or substances cannot be released at high temperature, and harm to human health and the environment is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resin material preparation, in particular to a high-temperature resistant insulating resin material. Background Art

[0002] Insulating resin material is a polymer composite material used for insulation, mainly composed of base resin, filling material, reinforcing material and additives. This material has the characteristics of good insulation, mechanical properties and chemical stability, so it has been widely used in the fields of electricity, electronics, aerospace, etc. Among them, epoxy resin, as a common high-temperature resistant resin material, is widely used in the electrical field due to its excellent insulation and mechanical properties. However, its high-temperature resistance is relatively limited, and the general operating temperature range is in the low to medium temperature range. In high-temperature environments, epoxy resin may experience performance degradation or failure. Therefore, in order to solve the problems of poor toughness and poor high-temperature resistance of traditional epoxy resin high-temperature resistant materials, it is necessary to study and improve them.

[0003] For example, the patent document with publication number CN118185242A discloses a high-temperature resistant resin material. The invention uses bisphenol A epoxy resin as the base material, and adds modified zirconium sulfide as a reinforcing modifier. The strength, toughness and high-temperature resistance of the modified epoxy resin are greatly improved. After experimental testing of the invention, it is found that the modified zirconium sulfide mixed with the epoxy resin can improve the strength, toughness and high-temperature resistance of the epoxy resin better than the performance of zirconium sulfide and diphenylchlorosilane alone.

[0004] However, the existing resin materials similar to the above applications still have the following shortcomings:

[0005] Existing high-temperature resistant epoxy resins use bisphenol A as the base material. Although the performance of modified epoxy resins has been greatly improved, especially the high-temperature resistance, bisphenol A epoxy resins are prone to release harmful gases or substances at high temperatures, which are harmful to human health and the environment. For example, bisphenol A in epoxy resins may precipitate at high temperatures, which has adverse effects on the human reproductive system. In addition, insulation, as one of the basic properties of resin materials, is directly related to its safety in use in the power field, but the insulation of existing resin materials still has room for improvement.

[0006] Therefore, it is urgent to improve this shortcoming. The present invention studies and improves the existing technology and its shortcomings, and provides a high temperature resistant insulating resin material. Summary of the invention

[0007] The object of the present invention is to provide a high temperature resistant insulating resin material to solve the problems raised in the above background technology.

[0008] To achieve the above object, the present invention provides the following technical solution: a high temperature resistant insulating resin material, wherein the preparation method of the resin material comprises the following steps:

[0009] S1. Raw material preparation:

[0010] Preparation of bisphenol F: prepare phenol and 37% formaldehyde aqueous solution as preparation raw materials, and 35% hydrochloric acid as a catalyst; under the action of the catalyst, phenol and formaldehyde undergo condensation reaction to generate bisphenol F;

[0011] Other raw materials: epichlorohydrin, NaOH (sodium hydroxide) solution, nanofiller, curing agent, etc.;

[0012] S2. Synthesis of bisphenol F type epoxy resin:

[0013] Pre-reaction: After bisphenol F is put into the pre-reaction kettle, NaOH solution is added, and then epichlorohydrin is introduced for preliminary reaction;

[0014] Polycondensation reaction: Add the remaining epichlorohydrin to the pre-reaction solution, and continue to add NaOH solution as a catalyst to carry out polycondensation reaction;

[0015] S3, modification treatment:

[0016] The nanofiller is added into pure water to be dispersed evenly, and then modified with epoxy groups to obtain epoxidized nanofiller, and then the epoxidized nanofiller is added into the reaction system of bisphenol F epoxy resin to carry out a mixing reaction to ensure that the nanoparticles are evenly dispersed in the resin;

[0017] S4, post-processing:

[0018] Through refining operations including distillation, filtration and washing, impurities and unreacted products in the reaction system are removed to obtain pure bisphenol F epoxy resin. The refined epoxy resin is then evenly mixed with a curing agent in a ratio of 10:5, and then cured to obtain a high-temperature resistant insulating resin material.

[0019] Furthermore, in step S1, the reaction temperature of the condensation reaction is controlled at 60-100° C. and is carried out at normal pressure (ie, about 1 atmosphere) or slightly higher than normal pressure to ensure product purity and yield.

[0020] Furthermore, in step S2, the reaction temperature of the pre-reaction is controlled at 60±5° C., and the reaction time is 8 to 10 hours, which can be adjusted according to the specific process.

[0021] Furthermore, in step S2, the reaction temperature of the polycondensation reaction is maintained at 60°C ± 2°C, the reaction time is adjusted according to the molecular weight and performance of the desired resin, and stirring is maintained during the reaction at a stirring speed of 180 r / min to ensure uniform reaction.

[0022] Furthermore, in step S3, the nanofiller is selected from one of nano-silicon, nano-zirconium oxide and nano-aluminum oxide.

[0023] Furthermore, in step S3, the nanofiller must be screened before use. The specific operations are as follows: first, a vibrating screen or an airflow screen is used for preliminary screening to remove coarse particles or agglomerates generated during production or transportation. Then, an ultrasonic vibrating screen or a centrifugal screen is used for further screening to promote the dispersion and separation of the nanoparticles. Then, a multi-stage screening system is used for grading treatment to gradually narrow the particle size range to obtain nanofillers that meet the requirements. Finally, a laser particle size analyzer, a scanning electron microscope (SEM) and other detection equipment are used to perform particle size detection and morphology observation on the screened nanofiller to ensure that the particle size distribution of the nanofiller is uniform and meets the predetermined particle size range requirements.

[0024] Furthermore, in step S3, the dispersion of the nanofiller is divided into an initial dispersion stage and a stable dispersion stage;

[0025] The stirring speed in the initial dispersion stage is controlled between 800 and 1200 r / min to break up the agglomeration between the nanofillers and promote their dispersion in water;

[0026] The stirring speed in the stable dispersion stage is controlled between 200 and 300 r / min. The stirring speed is reduced to maintain a stable dispersion state and avoid reagglomeration or foaming of the dispersed nanofillers.

[0027] Furthermore, in step S4, the refining operation is specifically as follows:

[0028] 1) Distillation: used to remove low-boiling-point volatile impurities in the reaction system, such as unreacted epichlorohydrin, formaldehyde, and possibly generated water. Specific steps: Place the reaction mixture in a distillation apparatus and slowly heat it to boiling. During the heating process, the temperature must be controlled to avoid excessively high temperatures that may cause thermal decomposition of the epoxy resin. According to the differences in boiling points of the components, fractions at different temperature ranges are collected. Low-boiling-point impurities will be evaporated first, while high-boiling-point epoxy resins will remain in the distillation kettle. At the same time, a thermometer and a fraction collector are used to monitor the distillation process to ensure that the collected fractions meet expectations.

[0029] 2) Filtration: used to remove insoluble solid impurities, such as catalyst residues, undissolved solid particles, etc. Specific steps: select filter materials according to the nature and particle size of the impurities, such as filter paper, glass sand core filter, etc., and then slowly pour the distilled resin solution into the filter to allow the solution to pass through the filter material, while the impurities are retained on the filter material. After the filtration is completed, wash the filter material with clean water or an appropriate solvent to remove the residual resin and impurities;

[0030] 3) Washing: used to further remove soluble impurities and unreacted products attached to the surface of the resin. Specific steps: place the filtered resin in a washing container, add a washing solvent that can dissolve impurities without affecting the performance of the resin, gently stir or shake the container to allow the washing solvent to fully contact with the resin to dissolve and remove impurities attached to the surface of the resin. Wash at least three times, and after each wash, remove the washing liquid and check the cleanliness of the resin. After washing, place the resin in a dryer for drying to remove residual washing solvent and moisture. The temperature and humidity must be controlled during the drying process to avoid thermal decomposition or moisture absorption of the resin.

[0031] Furthermore, in step S4, the curing agent is one of diethylenetriamine (DETA, which can react with bisphenol F epoxy resin at a lower temperature, but due to its high activity, it is necessary to control the curing reaction speed to avoid generating too much heat and causing the resin to burn), m-phenylenediamine (MDA, which has low volatility and high heat resistance. After reacting with bisphenol F epoxy resin, it can form a stable cross-linked structure to improve the heat resistance and mechanical strength of the resin), and phenolic resin (not only as a curing agent, but also as a modifier of epoxy resin. During the curing process, phenolic resin will undergo a cross-linking reaction with epoxy resin to form a complex network structure, thereby improving the heat resistance and corrosion resistance of the resin). Phenolic resin is preferably selected to induce a cross-linking reaction of the epoxy groups in the epoxy resin, so that it is transformed from a linear structure to a three-dimensional network structure.

[0032] The present invention provides a high temperature resistant insulating resin material, which has the following beneficial effects:

[0033] The present invention uses bisphenol F as a base material and adds a proper curing agent to increase the crosslinking density of the epoxy resin, making it stronger and more stable, thereby significantly improving the insulation performance of the epoxy resin, so that the prepared insulating resin material not only has excellent high temperature resistance, but also is not prone to a decrease in insulation performance under high temperature conditions, thereby effectively avoiding failure of the insulation structure of electrical equipment and reducing the risk of electrical faults such as leakage and short circuit. In addition, no harmful gases or substances will be released at high temperatures, thereby avoiding harm to human health and the environment.

[0034] The present invention improves the epoxy resin by adding nano-scale fillers, using fillers such as nano-silicon, nano-zirconium oxide and nano-aluminum oxide to fill the cavities and gaps in the epoxy resin, reduce internal defects, and thus improve its flame retardant and electrical properties; at the same time, the nano-scale fillers with polar groups also increase the surface energy of the epoxy resin and enhance its adhesion to the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a schematic diagram of the preparation process of a high temperature resistant insulating resin material of the present invention;

[0036] Figure 2 This is a performance test result table of a high temperature resistant insulating resin material of the present invention. DETAILED DESCRIPTION

[0037] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0038] Example 1

[0039] like Figure 1 As shown, a high temperature resistant insulating resin material, the preparation method of which includes:

[0040] S1. Raw material preparation:

[0041] Preparation of bisphenol F: Phenol and 37% formaldehyde aqueous solution are prepared as preparation raw materials, and 35% hydrochloric acid is used as a catalyst; under the action of the catalyst, phenol and formaldehyde undergo a condensation reaction to generate bisphenol F; the reaction temperature of the condensation reaction is controlled at 60 to 100° C., and the condensation reaction is carried out at normal pressure (i.e., about 1 atmosphere) or slightly higher than normal pressure to ensure product purity and yield;

[0042] Other raw materials: epichlorohydrin, NaOH (sodium hydroxide) solution, nanofiller, curing agent, etc.;

[0043] S2. Synthesis of bisphenol F type epoxy resin:

[0044] Pre-reaction: After bisphenol F is put into the pre-reaction kettle, NaOH solution is added, and then epichlorohydrin is introduced for preliminary reaction. The reaction temperature of the pre-reaction is controlled at 60±5°C, and the reaction time is 8 to 10 hours, which can be adjusted according to the specific process;

[0045] Polycondensation reaction: Add the remaining epichlorohydrin to the pre-reaction solution, and continue to add NaOH solution as a catalyst to carry out polycondensation reaction. The reaction temperature of the polycondensation reaction is maintained at 60°C ± 2°C. The reaction time is adjusted according to the molecular weight and performance of the required resin. Stirring is maintained during the reaction at a stirring speed of 180r / min to ensure uniform reaction.

[0046] S3, modification treatment:

[0047] The nanofiller is nanosilicon, which is evenly dispersed in pure water, and then modified with epoxy groups to obtain epoxidized nanosilicon, which is then added to a reaction system of bisphenol F epoxy resin to perform a mixing reaction to ensure that the nanoparticles are evenly dispersed in the resin.

[0048] Nano silicon must be screened before use. The specific operation is as follows: first, use a vibrating screen or airflow screen for preliminary screening to remove coarse particles or agglomerates generated during production or transportation. Then use an ultrasonic vibrating screen or centrifugal screen for further screening to promote the dispersion and separation of nanoparticles. Then use a multi-stage screening system for classification and gradually narrow the particle size range to obtain nano fillers that meet the requirements. Finally, use laser particle size analyzers, scanning electron microscopes (SEM) and other testing equipment to perform particle size detection and morphology observation on the screened nano fillers to ensure that the particle size distribution of the nano fillers is uniform and meets the predetermined particle size range requirements.

[0049] In addition, the dispersion of nanofillers is divided into the initial dispersion stage and the stable dispersion stage; the stirring speed in the initial dispersion stage is controlled at 1000r / min to break the agglomeration between nanofillers and promote their dispersion in water; the stirring speed in the stable dispersion stage is controlled at 250r / min, and the stirring speed is reduced to maintain a stable dispersion state to avoid the reagglomeration or foaming of the dispersed nanofillers;

[0050] S4, post-processing:

[0051] Through refining operations including distillation, filtration, and washing, impurities and unreacted products in the reaction system are removed to obtain pure bisphenol F epoxy resin, and then the refined epoxy resin is evenly mixed with phenolic resin in a ratio of 10:5 to induce a cross-linking reaction of epoxy groups in the epoxy resin, so that the linear structure is transformed into a three-dimensional network structure compound, thereby obtaining a high-temperature resistant insulating resin material;

[0052] The specific refining operations are as follows:

[0053] 1) Distillation: used to remove low-boiling-point volatile impurities in the reaction system, such as unreacted epichlorohydrin, formaldehyde, and possibly generated water. Specific steps: Place the reaction mixture in a distillation apparatus and slowly heat it to boiling. During the heating process, the temperature must be controlled to avoid excessively high temperatures that may cause thermal decomposition of the epoxy resin. According to the differences in boiling points of the components, fractions at different temperature ranges are collected. Low-boiling-point impurities will be evaporated first, while high-boiling-point epoxy resins will remain in the distillation kettle. At the same time, a thermometer and a fraction collector are used to monitor the distillation process to ensure that the collected fractions meet expectations.

[0054] 2) Filtration: used to remove insoluble solid impurities, such as catalyst residues, undissolved solid particles, etc. Specific steps: select filter materials according to the nature and particle size of the impurities, such as filter paper, glass sand core filter, etc., and then slowly pour the distilled resin solution into the filter to allow the solution to pass through the filter material, while the impurities are retained on the filter material. After the filtration is completed, wash the filter material with clean water or an appropriate solvent to remove the residual resin and impurities;

[0055] 3) Washing: used to further remove soluble impurities and unreacted products attached to the surface of the resin. Specific steps: place the filtered resin in a washing container, add a washing solvent that can dissolve impurities without affecting the performance of the resin, gently stir or shake the container to allow the washing solvent to fully contact with the resin to dissolve and remove impurities attached to the surface of the resin. Wash at least three times, and after each wash, remove the washing liquid and check the cleanliness of the resin. After washing, place the resin in a dryer for drying to remove residual washing solvent and moisture. The temperature and humidity must be controlled during the drying process to avoid thermal decomposition or moisture absorption of the resin.

[0056] Comparative Example 1

[0057] A resin material, which differs from Example 1 in that the bisphenol F preparation step in step S1 is replaced by commercially purchased bisphenol A (Wuhan Kangqiong Biopharmaceutical Technology Co., Ltd.), and the rest is the same as Example 1.

[0058] Comparative Example 2

[0059] A resin material, which differs from Example 1 in that the modification treatment in step S3 is omitted, and the rest is the same as Example 1.

[0060] Comparative Example 3

[0061] A resin material, which differs from Example 1 in that the phenolic resin added in step S4 is replaced by commercially purchased ethylenediamine (Wuhan Kangqiong Biopharmaceutical Technology Co., Ltd.), and the rest is the same as Example 1.

[0062] Experimental testing

[0063] In order to more clearly illustrate the content of the present invention, the resin materials prepared in Example 1 and Comparative Examples 1-3 were tested for performance. The test of insulation performance was based on GB / T 1408.1-2016, the test of high temperature resistance was based on GBT29602-2013, and the test of releasing harmful gases (or substances) at high temperature (180°C) was based on GB / T 27921-2011. The results are as follows: Figure 2 As shown:

[0064] Combination Figure 2It can be seen that the resin material prepared in Example 1 has higher insulation and better high temperature resistance, and releases less harmful gases (or substances) at high temperatures, which solves the problem that traditional epoxy resin high temperature resistant materials still release harmful gases (or substances) at high temperatures and have poor insulation performance.

[0065] The embodiments of the present invention are given for the purpose of illustration and description, and are not intended to be exhaustive or to limit the invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for specific uses.

Claims

1. A high temperature resistant insulating resin material, It is characterized in that The preparation method of the resin material comprises the following steps: S1. Raw material preparation: Preparation of bisphenol F: prepare phenol and 37% formaldehyde aqueous solution as preparation raw materials, and 35% hydrochloric acid as a catalyst; under the action of the catalyst, phenol and formaldehyde undergo condensation reaction to generate bisphenol F; Other raw materials: epichlorohydrin, NaOH solution, nanofiller, curing agent; S2. Synthesis of bisphenol F type epoxy resin: Pre-reaction: After bisphenol F is put into the pre-reaction kettle, NaOH solution is added, and then epichlorohydrin is introduced for preliminary reaction; Polycondensation reaction: Add the remaining epichlorohydrin to the pre-reaction solution, and continue to add NaOH solution as a catalyst to carry out polycondensation reaction; S3, modification treatment: The nanofiller is added into pure water to be dispersed evenly, and then modified with epoxy groups to obtain epoxidized nanofiller, and then the epoxidized nanofiller is added into the reaction system of bisphenol F epoxy resin to carry out a mixing reaction to ensure that the nanoparticles are evenly dispersed in the resin; S4, post-processing: Through refining operations including distillation, filtration and washing, impurities and unreacted products in the reaction system are removed to obtain pure bisphenol F epoxy resin. The refined epoxy resin is then evenly mixed with a curing agent in a ratio of 10:5, and then cured to obtain a high-temperature resistant insulating resin material.

2. A high temperature resistant insulating resin material according to claim 1, It is characterized in that In the step S1, the reaction temperature of the condensation reaction is controlled at 60-100° C. and is carried out under normal pressure to ensure product purity and yield.

3. The high temperature resistant insulating resin material according to claim 1, It is characterized in that In the step S2, the reaction temperature of the pre-reaction is controlled at 60±5° C., and the reaction time is 8 to 10 hours, which can be adjusted according to the specific process.

4. The high temperature resistant insulating resin material according to claim 1, It is characterized in that In the step S2, the reaction temperature of the polycondensation reaction is maintained at 60°C ± 2°C, the reaction time is adjusted according to the molecular weight and performance of the desired resin, and stirring is maintained during the reaction at a stirring speed of 180 r / min.

5. The high temperature resistant insulating resin material according to claim 1, It is characterized in that In step S3, the nano filler is selected from one of nano silicon, nano zirconium oxide and nano aluminum oxide.

6. A high temperature resistant insulating resin material according to claim 1, It is characterized in that In step S3, the nanofiller must be screened before use. The specific operation is as follows: first, a vibrating screen or an airflow screen is used for preliminary screening to remove coarse particles or agglomerates generated during production or transportation. Then, an ultrasonic vibrating screen or a centrifugal screen is used for further screening to promote the dispersion and separation of nanoparticles. Then, a multi-stage screening system is used for grading to gradually narrow the particle size range to obtain nanofillers that meet the requirements. Finally, a laser particle size analyzer and a scanning electron microscope are used to detect the particle size and observe the morphology of the nanofiller after screening to ensure that the particle size distribution of the nanofiller is uniform and meets the predetermined particle size range requirements.

7. The high temperature resistant insulating resin material according to claim 1, It is characterized in that In step S3, the dispersion of the nanofiller is divided into an initial dispersion stage and a stable dispersion stage; The stirring speed in the initial dispersion stage is controlled between 800 and 1200 r / min to break up the agglomeration between the nanofillers and promote their dispersion in water; The stirring speed in the stable dispersion stage is controlled between 200 and 300 r / min. The stirring speed is reduced to maintain a stable dispersion state and avoid reagglomeration or foaming of the dispersed nanofillers.

8. The high temperature resistant insulating resin material according to claim 1, It is characterized in that In step S4, the refining operation is specifically as follows: 1) Distillation: used to remove low-boiling-point volatile impurities in the reaction system. Specific steps: Place the reaction mixture in a distillation device, slowly heat it to boiling, and collect fractions at different temperature ranges according to the boiling point differences of each component. Low-boiling-point impurities will be evaporated first, while high-boiling-point epoxy resin will remain in the distillation kettle. At the same time, use a thermometer and a fraction collector to monitor the distillation process to ensure that the collected fractions meet expectations; 2) Filtration: used to remove insoluble solid impurities. Specific steps: select filter material according to the nature and particle size of the impurities, then slowly pour the distilled resin solution into the filter, let the solution pass through the filter material, and the impurities are trapped on the filter material; 3) Washing: used to further remove soluble impurities and unreacted products attached to the surface of the resin. The specific steps are as follows: place the filtered resin in a washing container, add a washing solvent that can dissolve impurities without affecting the performance of the resin, gently stir or shake the container to allow the washing solvent to fully contact the resin to dissolve and remove impurities attached to the surface of the resin. After washing, place the resin in a dryer for drying to remove residual washing solvent and moisture.

9. The high temperature resistant insulating resin material according to claim 1, It is characterized in that In step S4, the curing agent is one of diethylenetriamine, m-phenylenediamine and phenolic resin, which is used to initiate a cross-linking reaction of epoxy groups in the epoxy resin, thereby converting the linear structure into a three-dimensional network structure.

Citation Information

Patent Citations

  • High-temperature-resistant resin material