Polyether ester polyol as well as preparation method and application thereof

By introducing bisphenyl ring structure and esterification modification into the polyether polyol, polyether ester polyol was prepared as a pore opening agent, which solved the problem of insufficient mechanical properties and breathability of slow rebound polyurethane foam in the prior art. , achieving better opening effect and foam performance improvement.

CN118930838AActive Publication Date: 2024-11-12WANHUA CHEM GRP CO LTD

Patent Information

Application Number
CN202411196069.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The existing slow rebound polyurethane foam opener has problems such as poor fatigue, poor flexibility, poor breathability and poor opening effect in the application of high-end home furnishings, especially in high-density sponges.

Method used

The polyether polyol with bisphenyl ring structure is used to open the ring polymerization with hydrophobic alkylene oxide, and the long-chain fatty acid is added through esterification modification, and polyether ester polyol is prepared as a pore opening agent to enhance the foam. mechanical properties and breathability.

Benefits of technology

Significantly improves the mechanical properties of slow rebound foam (such as tear strength, tensile strength) and breathability, and increases the opening effect. It is suitable for high-end home products such as slow rebound U-shaped pillows, butterfly pillows and mattresses. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930838A_ABST
    Figure CN118930838A_ABST
Patent Text Reader

Abstract

The invention provides polyether ester polyol, a preparation method of the polyether ester polyol, a pore opening agent containing the polyether ester polyol, and application of the polyether ester polyol in preparation of slow-rebound polyurethane foam. The polyether ester polyol comprises a compound represented by (i), a compound represented by formula (ii), and an optional compound represented by formula (iii). The polyether ester polyol provided by the invention can provide a good hydrophobic and hole-breaking effect, effectively improves the defect of serious hole closing of slow-rebound foam, achieves the effect of foam hole opening, and ensures that the prepared slow-rebound foam has excellent air permeability # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention specifically relates to a polyether ester polyol for a slow rebound cell opening agent, a preparation method and an application thereof. Background Art

[0002] Slow-rebound polyurethane foam, also known as viscoelastic foam and memory sponge, is widely used in home furnishing fields such as slow-rebound mattresses and pillows due to its shape memory, energy absorption and shock absorption properties. It helps relieve human pressure and promote blood circulation. At present, there are two mainstream products in the slow-rebound market. The first type is glycerin-starting, high-proportion ethylene oxide and low-proportion propylene oxide ring-opening polymerization to prepare flatulence polyether products. The slow-rebound foam products prepared by this type of polyether have the disadvantages of poor fatigue resistance, poor flexibility, and poor slow rebound effect, and cannot be used in the field of high-end home furnishings. The second type is glycerin-starting, propylene oxide ring-opening polymerization to prepare small molecule polyether products. The slow-rebound foam products prepared by this type of polyether have excellent physical properties, but have the disadvantage of poor air permeability, and need to be used with a slow-rebound pore-opening agent. However, the pore-opening agent products currently on the market all have corresponding problems, such as... Defoaming agents such as organic paraffin or silicone have very narrow operating tolerances and are easy to destroy the foam stability of the sponge before it is fully risen, resulting in uneven sponge foam structure, coarse pores, and even foam collapse. Inorganic fillers such as calcium carbonate and barium sulfate have poor pore opening effects. Increasing the amount of addition will damage the sponge structure, resulting in decreased physical and mechanical properties such as tensile strength and tear strength. In addition, there are high molecular weight propylene oxide or butylene oxide homopolymer structure polyether polyols. This type of pore opening agent can achieve good pore opening efficiency in low-density sponges, but when the sponge density exceeds 60kg / m 3 The post-pore opening effect is minimal. Therefore, developing a pore opening agent product with excellent pore opening effect and without affecting the rationality of the slow rebound sponge's physical properties is currently a difficulty in this field.

[0003] CN102336900B discloses the use of a polyether polyol or a polyether polyester as a cell opener for slow-rebound polyurethane foam. A small molecular weight polyether polyol is used as an initiator and DMC is used as a catalyst to perform ring opening of alkylene oxide to prepare a cell opener with a structure of polyether polyol. Alternatively, a small molecular weight polyether polyol is used as an initiator and DMC is used as a catalyst to perform ring opening of alkylene oxide, and then a small molecule acid is used for esterification and end-capping to prepare a cell opener with a structure of polyether polyester. However, the cell opener prepared by this method is a polyether polyol or a polyether polyester, and the structure is only an ether bond structure or the ether bond is the main body and contains a very small amount of ester bond structure at the end. When used in slow-rebound foam, the cell opening effect is general and the mechanical properties of the slow-rebound foam are not improved. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the object of the present invention is to provide a polyether ester polyol, wherein a cell opening agent comprising the polyether ester polyol has excellent cell opening effect and can improve the mechanical properties of slow-rebound polyurethane foam.

[0005] Another object of the present invention is to provide a method for preparing the polyether ester polyol. In the method, a small molecule polyether polyol containing a double benzene ring structure is used as an initiator, and ring-opening polymerization is carried out with a hydrophobic alkylene oxide (propylene oxide, butylene oxide, etc.). The end is esterified with a long-chain fatty acid to further enhance the hydrophobic properties of the product. A polyether ester polyol for a cell opener is prepared. When used in a slow-rebound polyurethane foam, it is beneficial to open the foam cells and improve the mechanical properties of the foam.

[0006] Another object of the present invention is to provide a cell opener, which comprises the polyether ester polyol according to the present invention.

[0007] Another object of the present invention is to provide use of the polyether ester polyol according to the present invention in the preparation of slow-rebound polyurethane foam.

[0008] In order to achieve the above invention object, the present invention adopts the following technical solution:

[0009] According to a first aspect of the present invention, there is provided a polyetherester polyol comprising a compound represented by formula (i), a compound represented by formula (ii) and optionally a compound represented by formula (iii):

[0010]

[0011] wherein each m is the same or different, and each n is the same or different, and 0≤n≤60, 10≤m≤150;

[0012] R is:

[0013] R1 is a long-chain fatty acid residue, and the general structure is as follows: Wherein, X1 is an alkylene group or an alkylene group containing an unsaturated double bond, X2 is a hydroxyl group or a methyl group, and the total number of carbon atoms of the long-chain fatty acid is greater than or equal to 10, preferably 10 to 20.

[0014] In the polyetherester polyol, the molar proportion of the compound represented by formula (i) is 50% to 100%; the molar proportion of the compound represented by formula (ii) is 0% to 50%, preferably 5% to 50%; the molar proportion of the compound represented by formula (iii) is less than 5%.

[0015] According to a second aspect of the present invention, there is provided a method for preparing the polyether ester polyol, comprising the following steps:

[0016] Step 1): using a substance containing a double benzene ring structure as an initiator 1 and an alkylene oxide 1 as a polymerization monomer, a polymerization reaction is carried out under the action of a catalyst to obtain a polyether polyol prepolymer A;

[0017] Step 2): the polyether polyol prepolymer A in step 1) is subjected to a refining treatment to obtain a polyether polyol prepolymer B;

[0018] Step 3): using the polyether polyol prepolymer B in step 2) as the initiator 2 and the alkylene oxide 2 as the polymerization monomer, and polymerizing under the catalysis of DMC (double metal cyanide) to obtain polyether polyol C;

[0019] Step 4): the polyether polyol C and the long-chain fatty acid are uniformly mixed, and the polyether ester polyol is obtained by esterification reaction under the action of a catalyst.

[0020] Preferably, the initiator 1 in step 1) includes but is not limited to bisphenol A, bisphenol S and the like.

[0021] Preferably, when n is 0, alkylene oxide 1 is butylene oxide, and alkylene oxide 2 is butylene oxide; when n is not 0, alkylene oxide 1 is propylene oxide or propylene oxide and butylene oxide added sequentially, and alkylene oxide 2 is butylene oxide, wherein propylene oxide and butylene oxide added sequentially means that butylene oxide is added after the reaction of propylene oxide is completed.

[0022] Preferably, the catalyst in step 1) includes but is not limited to alkali metal hydroxides, alkaline earth metal hydroxides, and the like, such as potassium hydroxide, sodium hydroxide, cesium hydroxide, magnesium hydroxide, calcium hydride, and the like.

[0023] Preferably, the reaction temperature in step 1) is 90-130°C.

[0024] Preferably, the feeding time of the alkylene oxide 1 in step 1) is 1 to 10 hours.

[0025] Preferably, the mass ratio of the initiator 1 to the alkylene oxide 1 in step 1) is 1:1-30.

[0026] Preferably, the weight of the catalyst in step 1) accounts for 0.1% to 1% of the total weight of the initiator 1 and the alkylene oxide 1.

[0027] Preferably, in step 1), when the alkylene oxide 1 is propylene oxide and butylene oxide added sequentially, the mass ratio of propylene oxide to butylene oxide is 1:0.1-10.

[0028] Preferably, the refining in step 2) comprises acid neutralization, adsorption by adsorbent, vacuum dehydration and filtration.

[0029] Preferably, the acid in step 2) is selected from the group consisting of, but not limited to, phosphoric acid, sulfuric acid, nitric acid, hydrochloric acid, lactic acid, acetic acid or oxalic acid.

[0030] Preferably, in step 2), an acid is used to neutralize the system to a pH of 4-5.

[0031] Preferably, the adsorbent in step 2) is selected from but not limited to magnesium silicate, aluminum silicate, magnesium aluminum silicate, diatomaceous earth or white clay.

[0032] Preferably, the amount of the adsorbent in step 2) is 0.1-5% of the mass of the polyether polyol prepolymer A.

[0033] Preferably, the temperature of the acid neutralization in step 2) is 20-100°C.

[0034] Preferably, the adsorption temperature in step 2) is 80-120°C.

[0035] Preferably, the dehydration temperature in step 2) is 100-120°C.

[0036] Preferably, the dehydration time in step 2) is 1 to 10 hours.

[0037] Preferably, the dehydration pressure in step 2) is -0.095 MPa to 0 MPa.

[0038] Preferably, in step 2), the filter is selected from the group including but not limited to candle filters, sintered filter element filters, plate and frame filters, etc.

[0039] Preferably, the reaction temperature in step 3) is 120-160°C.

[0040] Preferably, the feeding time of the alkylene oxide in step 3) is 1 to 10 hours.

[0041] Preferably, the mass ratio of the polyether polyol prepolymer B to the alkylene oxide in step 3) is 1:1-20.

[0042] Preferably, the amount of DMC (double metal cyanide) used in step 3) is 0.002% to 0.1% of the mass of the polyether polyol prepolymer B.

[0043] Preferably, the long-chain fatty acid in step 4) has the following structure:

[0044]

[0045] Wherein X1 is an alkylene group or an alkylene group containing an unsaturated double bond, X2 is a hydroxyl group or a methyl group, and the total number of carbon atoms of the long-chain fatty acid is greater than or equal to 10, preferably 10 to 20; more preferably, the long-chain fatty acid is selected from but not limited to one or more of ricinoleic acid, linolenic acid, linoleic acid, arachidic acid, eleostearic acid, 12,13-epoxyoleic acid and oleic acid.

[0046] Preferably, the catalyst in step 4) includes but is not limited to isobutyl titanate, isopropyl titanate, n-butyl titanate, triethylamine, trimethylamine and the like.

[0047] Preferably, the reaction temperature in step 4) is 180-260°C.

[0048] Preferably, the molar ratio of the polyether polyol C to the long-chain fatty acid in step 4) is 1:0.5-1.

[0049] Preferably, the mass ratio of the long-chain fatty acid to the catalyst in step 4) is 1:0.001-0.1.

[0050] It should be noted that in the present application, polyether polyol prepolymer A, polyether polyol prepolymer B and polyether polyol C are all intermediate products of the final product polyether ester polyol of the present invention, and those skilled in the art can determine its structure based on the final product polyether ester polyol and the reaction steps.

[0051] Specifically, the polyether polyol prepolymer A and the polyether polyol prepolymer B have the same structure.

[0052] When n is 0, the structural formula of polyether polyol prepolymer A and polyether polyol prepolymer B is H-(OC4H8) p -R-(C4H8O) p -H; the structural formula of polyether polyol C is H-(OC4H8) m -R-(C4H8O) m -H;

[0053] When n is not 0, the structural formula of polyether polyol prepolymer A and polyether polyol prepolymer B is H-(OC4H8) k -(OC3H6) n -R-(C3H6O) n -(C4H8O) k -H, the structural formula of polyether polyol C is H-(OC4H8) m -(OC3H6) n -R-(C3H6O) n -(C4H8O) m -H;

[0054] Wherein, R, n and m are defined as above, p is 1 to 10, and p is less than m; k is 0 to 10, and k is less than m.

[0055] According to a third aspect of the present invention, a cell opener is provided, which comprises the polyether ester polyol according to the present invention.

[0056] According to a fourth aspect of the present invention, there is provided use of the polyether ester polyol according to the present invention in preparing a slow-rebound polyurethane foam.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] The slow-rebound cell-opening agent polyether ester polyol of the present invention contains a double benzene ring structure in its structure. When used in the slow-rebound foam, it provides sufficient rigidity and effectively increases the mechanical properties (tear strength, tensile strength, etc.) of the slow-rebound foam. When preparing the slow-rebound foam, the addition amount of the commercially available common slow-rebound cell-opening agent polyether polyol is at most 5 parts by weight relative to 100 parts by weight of the raw material. If the amount is further increased, the mechanical properties of the slow-rebound foam will be seriously reduced. The slow-rebound cell-opening agent polyether ester polyol of the present invention can not only be added in a large amount, but also improves the mechanical properties of the prepared slow-rebound foam.

[0059] The slow-rebound cell-opening agent polyether ester polyol of the present invention contains a super-hydrophobic fatty acid chain segment in its terminal structure. When used in the slow-rebound foam, it can provide a good hydrophobic cell-breaking effect, effectively improving the serious disadvantage of the slow-rebound foam closed cells, achieving the effect of foam cell opening, and ensuring that the prepared slow-rebound foam has excellent air permeability. When used in home furnishing fields such as slow-rebound U-shaped pillows, butterfly pillows and mattresses, it provides consumers with good comfort and health. DETAILED DESCRIPTION

[0060] In order to better understand the technical solution of the present invention, the following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.

[0061] It should be noted that in the embodiments and comparative examples of the present invention, since the conversion rate of the etherification reaction in the presence of alkali or DMC catalyst is as high as 99% to 100%, the values ​​of n and m in the polyetherester compound can be roughly calculated based on the feed ratio.

[0062] Example 1

[0063] Add 500 g of bisphenol A and 15 g of potassium hydroxide into a high-pressure reactor, fully replace with nitrogen 10 times, continuously introduce 2500 g of propylene oxide at 120° C. for 5 hours, and ripen for 1 hour to prepare polyether polyol prepolymer A; add phosphoric acid into the reactor, stir at 80° C. for 1 hour, adjust the pH to 4-5, add 25 g of magnesium silicate, stir at 90° C. for 1 hour, heat to 110° C., vacuum dehydrate at -0.095 MPa for 5 hours, and filter through a candle filter to obtain refined polyether polyol prepolymer B;

[0064] Add 2000 g of polyether polyol prepolymer B and 1 g of DMC catalyst into the autoclave, fully replace with nitrogen 10 times, and continuously introduce 10000 g of butylene oxide within 10 h at 160° C. under stirring, and ripen for 1 h to prepare polyether polyol C;

[0065] Add 436g of ricinoleic acid and 43.6g of isobutyl titanate into the reactor, and carry out esterification reaction at 260°C for 10h, maintain 260°C, and vacuum dehydrate at -0.095MPa for 2h to prepare a slow rebound cell-opening agent polyether ester polyol. The hydroxyl value is 13.98mgKOH / g, and the molar proportion of polyether polyols capped with ricinoleic acid residues on only one side is 89.2% by nuclear magnetic resonance, the molar proportion of polyether polyols not capped with ricinoleic acid residues on both sides is 7.7%, and the molar proportion of polyether polyols capped with ricinoleic acid residues on both sides is 3.1%.

[0066] Example 2

[0067] Add 500 g of bisphenol S and 15 g of sodium hydroxide into a high-pressure reactor, fully replace with nitrogen 10 times, continuously introduce 500 g of propylene oxide at 130° C. for 2 hours, mature for 10 minutes, and then continuously introduce 500 g of butylene oxide within 2 hours and mature for 1 hour to prepare polyether polyol prepolymer A; add sulfuric acid into the reactor, stir at 50° C. for 1 hour, adjust the pH to 4-5, add 30 g of diatomaceous earth, stir at 80° C. for 1 hour, heat to 120° C., vacuum dehydrate at -0.080 MPa for 8 hours, and filter through a plate and frame filter to obtain refined polyether polyol prepolymer B;

[0068] Add 750 g of polyether polyol prepolymer B and 0.75 g of DMC catalyst into the autoclave, fully replace with nitrogen 10 times, and continuously introduce 11250 g of butylene oxide within 5 h at 150 ° C with stirring, and ripen for 1 h to prepare polyether polyol C;

[0069] Add 168g of linolenic acid and 8.4g of triethylamine into the reactor, carry out esterification reaction at 240°C for 10h, maintain 240°C, and vacuum dehydrate at -0.095MPa for 2h to prepare a slow rebound cell-opening agent polyether ester polyol. The hydroxyl value is 6.87mgKOH / g, and the molar proportion of the polyether polyol capped with linolenic acid residues on only one side is 57.3%, the molar proportion of the polyether polyol not capped with linolenic acid residues on both sides is 41.8%, and the molar proportion of the polyether polyol capped with linolenic acid residues on both sides is 0.9%.

[0070] Example 3

[0071] Add 500 g of bisphenol A and 15 g of potassium hydroxide into a high-pressure reactor, fully replace with nitrogen 10 times, continuously introduce 2500 g of butylene oxide at 120° C. for 5 hours, and ripen for 1 hour to prepare polyether polyol prepolymer A; add phosphoric acid into the reactor, stir at 90° C. for 1 hour, adjust the pH to 4-5, add 25 g of magnesium silicate, stir at 100° C. for 1 hour, heat to 110° C., vacuum dehydrate at -0.095 MPa for 5 hours, and filter through a candle filter to obtain refined polyether polyol prepolymer B;

[0072] Add 2000 g of polyether polyol prepolymer B and 1 g of DMC catalyst into the autoclave, fully replace with nitrogen 10 times, and continuously introduce 10000 g of butylene oxide within 10 h at 160° C. under stirring, and ripen for 1 h to prepare polyether polyol C;

[0073] Add 400g of ricinoleic acid and 35.0g of isobutyl titanate into the reactor, carry out esterification reaction at 260°C for 10h, maintain 260°C, and vacuum dehydrate at -0.095MPa for 2h to prepare a slow rebound cell-opening agent polyether ester polyol. The hydroxyl value is 14.10mgKOH / g, and the molar proportion of polyether polyols capped with ricinoleic acid residues on only one side is 88.3% by nuclear magnetic resonance, the molar proportion of polyether polyols not capped with ricinoleic acid residues on both sides is 10.2%, and the molar proportion of polyether polyols capped with ricinoleic acid residues on both sides is 1.5%.

[0074] Example 4

[0075] Add 500 g of bisphenol A and 15 g of potassium hydroxide into a high-pressure reactor, fully replace with nitrogen 10 times, continuously introduce 1500 g of butylene oxide at 120° C. for 5 hours, and ripen for 1 hour to prepare polyether polyol prepolymer A; add phosphoric acid into the reactor, stir at 90° C. for 1 hour, adjust the pH to 4-5, add 25 g of magnesium silicate, stir at 100° C. for 1 hour, heat to 110° C., vacuum dehydrate at -0.095 MPa for 5 hours, and filter through a candle filter to obtain polyether polyol prepolymer B;

[0076] Add 1000 g of polyether polyol prepolymer B and 0.8 g of DMC catalyst into the autoclave, fully replace with nitrogen 10 times, and continuously introduce 1000 g of butylene oxide within 1 h at 150° C. under stirring, and ripen for 1 h to prepare polyether polyol C;

[0077] 326g of ricinoleic acid and 26.0g of isobutyl titanate were added into the reactor, and the esterification reaction was carried out at 260°C for 10h, and the temperature was maintained at 240°C, and vacuum dehydration was carried out at -0.095MPa for 2h to prepare a slow rebound cell-opening agent polyether ester polyol. The hydroxyl value was determined to be 53.18mgKOH / g, and the molar proportion of the polyether polyol capped with ricinoleic acid residues on only one side was 87.6% by nuclear magnetic resonance, the molar proportion of the polyether polyol not capped with ricinoleic acid residues on both sides was 7.7%, and the molar proportion of the polyether polyol capped with ricinoleic acid residues on both sides was 4.7%.

[0078] Example 5

[0079] Add 500 g of bisphenol A and 50.75 g of potassium hydroxide into a high-pressure reactor, fully replace with nitrogen 10 times, continuously introduce 14000 g of propylene oxide at 100° C. for 10 hours, and ripen for 1 hour to prepare polyether polyol prepolymer A; add phosphoric acid into the reactor, stir at 90° C. for 1 hour, adjust the pH to 4-5, add 145 g of magnesium silicate, stir at 100° C. for 1 hour, heat to 110° C., vacuum dehydrate at -0.095 MPa for 5 hours, and filter through a candle filter to obtain polyether polyol prepolymer B;

[0080] Add 661 g of polyether polyol prepolymer B and 0.17 g of DMC catalyst into the autoclave, fully replace with nitrogen 10 times, and continuously introduce 2091 g of butylene oxide within 10 h at 150° C. under stirring, and ripen for 1 h to prepare polyether polyol C;

[0081] Add 21g of ricinoleic acid and 2.1g of isobutyl titanate into the reactor, and carry out esterification reaction at 260°C for 10h, maintain 260°C, and vacuum dehydrate at -0.095MPa for 2h to prepare a slow rebound cell-opening agent polyether ester polyol. The hydroxyl value is 4.08mgKOH / g, and the molar proportion of polyether polyols capped with ricinoleic acid residues on only one side is 65.2% by nuclear magnetic resonance, the molar proportion of polyether polyols not capped with ricinoleic acid residues on both sides is 33.6%, and the molar proportion of polyether polyols capped with ricinoleic acid residues on both sides is 1.2%.

[0082] Comparative Example 1

[0083] The synthesis method is the same as that of Example 1, except that only polyether polyol C is prepared without using ricinoleic acid for esterification modification. The hydroxyl value of the product is 14.52 mgKOH / g, and the molar proportion of the polyether polyol not capped by ricinoleic acid residues on both sides is 100% by nuclear magnetic resonance.

[0084] Comparative Example 2

[0085] The initiator bisphenol A in Example 1 was replaced with polyether WANOL PPG230 (produced by Wanhua Chemical Group Co., Ltd., with a functionality of 2 and a hydroxyl value of 490 mgKOH / g), and the other conditions remained unchanged. The hydroxyl value of the product was determined to be 13.23 mgKOH / g, and the molar proportion of the polyether polyol capped with ricinoleic acid residues on only one side was 90.3% by nuclear magnetic resonance, the molar proportion of the polyether polyol not capped with ricinoleic acid residues on both sides was 6.5% by molar proportion of the polyether polyol capped with ricinoleic acid residues on both sides was 3.2% by molar proportion.

[0086] Comparative Example 3

[0087] Except that the amount of ricinoleic acid added in Example 1 was replaced with 850 g, the other conditions remained unchanged. The hydroxyl value was determined to be 13.82 mgKOH / g, and the molar proportion of the polyether polyol capped with ricinoleic acid residues on only one side was 5.3% by nuclear magnetic resonance, the molar proportion of the polyether polyol not capped with ricinoleic acid residues on both sides was 1.2%, and the molar proportion of the polyether polyol capped with ricinoleic acid residues on both sides was 93.5%.

[0088] Comparative Example 4

[0089] Add 500 g of bisphenol A and 15 g of potassium hydroxide into a high-pressure reactor, fully replace with nitrogen 10 times, continuously introduce 2500 g of propylene oxide at 120° C. for 5 hours, and ripen for 1 hour to prepare polyether polyol prepolymer A; add phosphoric acid into the reactor, stir at 80° C. for 1 hour, adjust the pH to 4-5, add 25 g of magnesium silicate, stir at 90° C. for 1 hour, heat to 110° C., vacuum dehydrate at -0.095 MPa for 5 hours, and filter through a candle filter to obtain refined polyether polyol prepolymer B;

[0090] Add 600g of ricinoleic acid and 30.5g of isobutyl titanate into the reactor, carry out esterification reaction at 260°C for 10h, maintain 260°C, and vacuum dehydrate at -0.095MPa for 2h to prepare a slow rebound cell-opening agent polyether ester polyol. The hydroxyl value is 68.9mgKOH / g, and the molar proportion of polyether polyols capped with ricinoleic acid residues on only one side is 85.3% by nuclear magnetic resonance, the molar proportion of polyether polyols not capped with ricinoleic acid residues on both sides is 12.0%, and the molar proportion of polyether polyols capped with ricinoleic acid residues on both sides is 2.7%.

[0091] Application performance testing:

[0092] The slow-rebound polyurethane foam was prepared using the following components:

[0093] MDI (diphenylmethane diisocyanate, produced by Wanhua Chemical Group Co., Ltd.);

[0094] POP 2045 (polymer polyol, produced by Wanhua Chemical Group Co., Ltd.)

[0095] WANOL S3007 (polyether polyol, produced by Wanhua Chemical Group Co., Ltd.);

[0096] WANOL F3156D (polyether polyol, produced by Wanhua Chemical Group Co., Ltd.);

[0097] Polyurethane foaming additives include: silicone oil HW0193, Y10366, catalyst A33, T9, desalted water;

[0098] Slow rebound opening agent SKC1900 (produced by SK Group of South Korea).

[0099] The production process of slow rebound foam is as follows:

[0100] Add the polyether polyol, polymer polyol, pore opener (polyether ester polyol prepared in the examples or comparative examples), water, silicone oil additive, and foaming catalyst shown in Table 1 into a beaker in sequence. Control the material temperature at 22-25°C and stir evenly with an electric stirrer at a speed of 4000r / min. At room temperature of 20-30°C, quickly add isocyanate, stir for 6-8s, and pour the mixture into a foaming box for free foaming. Make foam of 45cm×45cm×20cm specifications for physical property testing. The test is carried out after aging at room temperature for 72h.

[0101] Table 1: The formula and properties of slow-rebound polyurethane foam are as follows:

[0102]

[0103]

[0104] Note: The test methods for the physical properties of slow-rebound polyurethane foam are as follows: Tensile strength: Test reference GB 6344-2008;

[0105] Tear strength: Test reference GB 10808-2006;

[0106] Elongation at break: Test reference GB 6344-2008;

[0107] 65% indentation hardness: test reference GB 10807-2006;

[0108] Compression set: Test reference GB 6669-2008;

[0109] Air permeability: Test reference GB / T 5453-1997;

[0110] Slow rebound time: compress the foam to the lowest height with force, and record the foam recovery time after removing the external force.

[0111] As can be seen from the above table, the mechanical properties (tensile strength, tear strength, elongation at break, etc.) and air permeability of the slow-rebound polyurethane foam prepared by the embodiment of the present invention are significantly superior to those of the slow-rebound foam prepared by the comparative example and the commercially available cell-opening agent products, indicating that the slow-rebound cell-opening agent polyether ester polyol synthesized by the present invention has good practical value in the field of slow-rebound polyurethane foam.

[0112] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Those skilled in the art will appreciate that, under the guidance of this specification, some modifications or adjustments may be made to the present invention. These modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A polyetherester polyol comprising a compound represented by formula (i), a compound represented by formula (ii), and optionally a compound represented by formula (iii): in, Each m is the same or different, and each n is the same or different, and 0≤n≤60, 10≤m≤150; R is: R1 is a long-chain fatty acid residue, and the general structure is as follows: Wherein, X1 is an alkylene group or an alkylene group containing an unsaturated double bond, X2 is a hydroxyl group or a methyl group, and the total number of carbon atoms of the long-chain fatty acid is greater than or equal to 10, preferably 10 to 20.

2. The polyetherester polyol according to claim 1, wherein The molar proportion of the compound represented by formula (i) is 50% to 100%; the molar proportion of the compound represented by formula (ii) is 0% to 50%, preferably 5% to 50%; the molar proportion of the compound represented by formula (iii) is less than 5%.

3. A method for preparing the polyether ester polyol according to claim 1 or 2, comprising the following steps: Step 1): using a substance containing a double benzene ring structure as an initiator 1 and an alkylene oxide 1 as a polymerization monomer, a polymerization reaction is carried out under the action of a catalyst to obtain a polyether polyol prepolymer A; Step 2): the polyether polyol prepolymer A in step 1) is subjected to a refining treatment to obtain a refined polyether polyol prepolymer B; Step 3): using the polyether polyol prepolymer B in step 2) as the initiator 2 and the alkylene oxide 2 as the polymerization monomer, and polymerizing under the catalysis of double metal cyanide to obtain polyether polyol C; Step 4): the polyether polyol C and the long-chain fatty acid are uniformly mixed, and the polyether ester polyol is obtained by esterification reaction under the action of a catalyst.

4. The method for preparing polyetherester polyol according to claim 3, wherein: The initiator 1 in step 1) is bisphenol A or bisphenol S; and / or When n is 0, alkylene oxide 1 is butylene oxide, and alkylene oxide 2 is butylene oxide; when n is not 0, alkylene oxide 1 is propylene oxide or propylene oxide and butylene oxide added in sequence, and alkylene oxide 2 is butylene oxide, wherein propylene oxide and butylene oxide added in sequence means that butylene oxide is added after the reaction of propylene oxide is completed; and / or The catalyst in step 1) is an alkali metal hydroxide or an alkaline earth metal hydroxide, such as potassium hydroxide, sodium hydroxide, cesium hydroxide, magnesium hydroxide or calcium hydride; and / or The reaction temperature in step 1) is 90-130°C; and / or The feeding time of the alkylene oxide 1 in step 1) is 1 to 10 hours; and / or The mass ratio of the initiator 1 to the alkylene oxide 1 in step 1) is 1:1 to 30; and / or The weight of the catalyst in step 1) accounts for 0.1% to 1% of the sum of the weights of the initiator 1 and the alkylene oxide 1; and / or In step 1), when the alkylene oxide 1 is propylene oxide and butylene oxide added in sequence, the mass ratio of propylene oxide to butylene oxide is 1:0.1-10; and / or The purification in step 2) includes neutralization with acid, adsorption with adsorbent, vacuum dehydration and filtration.

5. The method for preparing polyether ester polyol according to claim 4, wherein: The acid in step 2) is selected from phosphoric acid, sulfuric acid, nitric acid, hydrochloric acid, lactic acid, acetic acid or oxalic acid; and / or In step 2), acid is used to neutralize the system to a pH of 4 to 5; and / or The adsorbent in step 2) is selected from magnesium silicate, aluminum silicate, magnesium aluminum silicate, diatomaceous earth or clay; and / or The amount of the adsorbent in step 2) is 0.1% to 5% of the mass of the polyether polyol prepolymer A; and / or The temperature of the acid neutralization in step 2) is 20 to 100° C.; and / or The adsorption temperature in step 2) is 80-120°C; and / or The dehydration temperature in step 2) is 100-120°C; and / or The dehydration time in step 2) is 1 to 10 hours; and / or The dehydration pressure in step 2) is -0.095 MPa to 0 MPa; and / or The filter in step 2) is selected from candle filters, sintered filter element filters and plate and frame filters.

6. The method for preparing polyetherester polyol according to any one of claims 3 to 5, wherein: The reaction temperature in step 3) is 120-160°C; and / or The feeding time of the alkylene oxide 2 in step 3) is 1 to 10 hours; and / or The mass ratio of the polyether polyol prepolymer B to the alkylene oxide 2 in step 3) is 1:1 to 20; and / or The amount of double metal cyanide used in step 3) is 0.002% to 0.1% of the mass of the polyether polyol prepolymer B.

7. The method for preparing polyetherester polyol according to any one of claims 3 to 6, wherein The long-chain fatty acid in step 4) has the following structure: in, X1 is an alkylene group or an alkylene group containing an unsaturated double bond, X2 is a hydroxyl group or a methyl group, and the total number of carbon atoms of the long-chain fatty acid is greater than or equal to 10, preferably 10 to 20; and / or The catalyst in step 4) is selected from isobutyl titanate, isopropyl titanate, n-butyl titanate, triethylamine or trimethylamine; and / or The reaction temperature in step 4) is 180-260°C; and / or The molar ratio of polyether polyol C to long-chain fatty acid in step 4) is 1:0.5-1; and / or The mass ratio of the long-chain fatty acid to the catalyst in step 4) is 1:0.001-0.

1.

8. The method for preparing polyether ester polyol according to claim 7, wherein The long-chain fatty acid is selected from one or more of ricinoleic acid, linolenic acid, linoleic acid, arachidic acid, eleostearic acid, 12,13-epoxyoleic acid and oleic acid. 9 . A cell opener comprising the polyether ester polyol according to claim 1 .

10. Use of the polyetherester polyol according to claim 1 or 2 in the preparation of slow-rebound polyurethane foam.

Citation Information

Patent Citations

  • Application of polyether polyols or polyether polyesters as opening agents for slow-rebound polyurethane foams

    CN102336900B

  • Toner and method of producing toner

    CN103389628A

  • Polyether polyol for self-trepanning low-temperature soft slow-rebound mattress foam, preparation method of polyether polyol, slow-rebound foam, and preparation method of slow-rebound foam

    CN110628009A

  • Carbon dioxide-based polycarbonate ether polyol for slow-rebound polyurethane foam, and preparation method thereof

    CN113773483A

  • Polyether polyol as well as preparation method and application thereof

    CN113881031A

Cited By

  • Preparation method of polyether ester defoaming agent

    CN120504825A

  • Preparation method of propoxylated bisphenol A

    CN121021271A

  • A process for the preparation of propoxylated bisphenol a

    CN121021271B