Preparation of copper (II) catalyst and application of copper (II) catalyst in catalyzing synthesis of polyvinyl chloride

Copper (II) catalyst was prepared through solvent thermal synthesis, and its hexagonal mesh structure was used as a catalyst to solve the environmental and energy consumption problems during vinyl chloride synthesis, and achieve efficient, mercury-free polyvinyl chloride production, providing Stable catalytic performance.

CN118930879AActive Publication Date: 2024-11-12SHAANXI SCI TECH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410986880.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing catalysts have environmental and energy consumption problems in the vinyl chloride synthesis process, and traditional catalysts are difficult to achieve efficient and mercury-free polyvinyl chloride production.

Method used

The copper (II) catalyst was prepared by solvent-thermal synthesis conditions, and coordinated with 3-PDCA and 4,4'-bipyridine ligands through 1 copper ion, and used 2 bridged ligands to form a hexagonal network structure. The C18H14CuN3O6 catalyst is formed as a catalyst for the synthesis of vinyl chloride and acetylene.

Benefits of technology

High conversion and high selectivity are achieved, filling the industry gap in mercury-free polyvinyl chloride production, and providing a stable new coordination polymer catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930879A_ABST
    Figure CN118930879A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalysts, in particular to preparation of a copper (II) catalyst and application of the copper (II) catalyst in catalyzing synthesis of polyvinyl chloride. One copper ion is coordinated with a 1-(3-carboxyl phenyl)-5-methyl-4-oxo-1, 4-dihydropyridazine-3-carboxyl (3-PDCA) ligand and a 4, 4 '-dipyridyl ligand at the same time, and a special hexagonal net structure is formed by utilizing two bridging ligands, so that the copper (II) catalyst with a novel structure is obtained. The copper (II) catalyst has the characteristics of higher acetylene conversion rate and better stability, more importantly, the development of a novel coordination polymer catalyst instead of a traditional catalyst becomes possible, and the industrial blank of calcium carbide method polyvinyl chloride mercuration-free production can be filled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to the preparation of a copper (II) catalyst and its application in catalyzing the synthesis of polyvinyl chloride. Background Art

[0002] Vinyl chloride is an important industrial intermediate, widely used in the preparation of polyvinyl chloride (PVC) and other processes. Its synthesis is usually obtained by the chlorination reaction of ethylene and chlorine, but this method has environmental and energy consumption problems. Catalytic synthesis of vinyl chloride has become an important way to reduce environmental impact and improve energy efficiency. Commonly used catalysts include metal chlorides, oxides or organic coordination polymers containing metal centers, which can promote the selective reaction of ethylene and chlorine, and improve the yield and product purity of vinyl chloride. In addition, optimizing reaction conditions such as temperature, pressure and reactant ratio also has a significant effect on the efficiency and selectivity of the reaction. Therefore, research and development of efficient and environmentally friendly catalytic systems are of great significance for the industrial production of vinyl chloride.

[0003] The present invention adopts solvent thermal synthesis conditions to synthesize a copper (II) catalyst, and tests the catalytic vinyl chloride synthesis performance thereof. The copper (II) catalyst exhibits good acetylene hydrochlorination activity as a catalyst, and its high acetylene conversion rate and high vinyl chloride selectivity are likely to become a mainstream new coordination polymer catalyst for synthesizing vinyl chloride. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a preparation method of a copper (II) catalyst and its application in catalyzing the synthesis of polyvinyl chloride in view of the shortcomings of the above-mentioned prior art. The temperature of the solvent thermal reaction is program-controlled, a copper ion is coordinated with a 3-PDCA ligand and a 4,4'-bipyridine ligand at the same time, and a special hexagonal network structure is formed by using two bridging ligands to prepare a copper (II) catalyst C 18 H 14 CuN3O6, whose coordination polymer has good stability, is used as a catalyst in the preparation process of vinyl chloride from hydrogen chloride and acetylene. Its high conversion rate and high selectivity are likely to become the mainstream mercury-free catalyst for the synthesis of polyvinyl chloride.

[0005] In order to solve the above technical problems, the present invention provides a copper (II) catalyst, the molecular formula of which is C 18 H 14 CuN3O6.

[0006] The present invention provides a method for preparing the above copper (II) catalyst, comprising the following steps:

[0007] S1. Add 3-PDCA ligand and 4,4'-bipyridine ligand into acetonitrile and stir evenly to obtain acetonitrile suspension;

[0008] S2, dissolving copper nitrate trihydrate in deionized water and stirring evenly to obtain a copper nitrate trihydrate solution;

[0009] S3. Add the copper nitrate trihydrate solution prepared in S2 to the acetonitrile suspension prepared in S1, stir evenly, and after solvent thermal reaction, filter, wash and vacuum dry in sequence to obtain a copper (II) catalyst.

[0010] According to the preparation method provided by the present invention, the molar volume ratio of the 3-PDCA ligand, the 4,4'-bipyridine ligand and the acetonitrile in S1 is 0.05 mmol: 0.05 mmol: 2 to 4 mL.

[0011] The preparation method provided by the present invention is characterized in that the molar volume ratio of the copper nitrate trihydrate and deionized water in S2 is 0.1 mmol: 1-3 mL;

[0012] According to the preparation method provided by the present invention, the temperature control procedure of the solvent thermal reaction in S3 is: heating to 110°C and maintaining for 48 hours, then cooling to room temperature, the heating rate of the heating is 0.1°C / min, and the cooling rate of the cooling is 0.1°C / min.

[0013] According to the preparation method provided by the present invention, the volume ratio of the hydrated copper nitrate solution and the acetonitrile suspension in S3 is 1:1.

[0014] According to the preparation method provided by the present invention, the detergent selected for washing in S3 is a mixed detergent of acetonitrile and deionized water, and the volume ratio of acetonitrile to deionized water in the mixed detergent is 1:1.

[0015] According to the preparation method provided by the present invention, the stirring speed in S1, S2 and S3 is 1200 rpm.

[0016] The present invention also provides an application of the copper (II) catalyst, wherein the copper (II) catalyst is used for catalyzing the synthesis of vinyl chloride.

[0017] Compared with the prior art, the present invention has the following advantages:

[0018] (1) The present invention coordinates a copper ion with a 3-PDCA ligand and a 4,4'-bipyridine ligand at the same time, and uses two bridging ligands to form a special hexagonal network structure, thereby obtaining a copper (II) catalyst C with a novel structure. 18 H 14 CuN3O6, the copper (II) catalyst can be used as a catalyst in the process of synthesizing vinyl chloride from hydrogen chloride and acetylene.

[0019] (2) The copper (II) catalyst in the present invention has high acetylene conversion rate and good stability. The development of new coordination polymer catalysts to replace traditional catalysts becomes possible, which can fill the industry gap in mercury-free production of polyvinyl chloride by calcium carbide process. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Schematic diagram of the molecular structure of copper (II) catalyst;

[0021] Figure 2 It is the network structure diagram of copper (II) catalyst;

[0022] Figure 3 This is a performance diagram of acetylene conversion and polyethylene selectivity of copper (II) catalyst. DETAILED DESCRIPTION

[0023] Example 1

[0024] This embodiment provides a method for preparing a copper (II) catalyst, comprising the following steps:

[0025] S1, add 0.05 mmol of 1-(3-carboxyphenyl)-5-methyl-4-oxo-1,4-dihydropyridazine-3-carboxyl (3-PDCA) ligand and 0.05 mmol of 4,4'-bipyridine ligand into 3 mL of acetonitrile, and stir at a speed of 1200 rpm to obtain an acetonitrile suspension;

[0026] S2, take 0.1mmol of copper nitrate trihydrate and dissolve it in 3mL of deionized water, stir it evenly at a speed of 1200rpm to obtain a copper nitrate trihydrate solution;

[0027] S3, adding the copper nitrate trihydrate solution prepared in S2 to the acetonitrile suspension prepared in S1, stirring at a rotation speed of 1200 rpm to obtain a mixed suspension, wherein the volume ratio of the copper nitrate trihydrate solution to the acetonitrile suspension is 1:1, placing the mixed suspension in a high-pressure reactor, and performing a solvothermal reaction under programmed temperature control, wherein the specific temperature control program is: heating to 110°C and maintaining for 72 hours, and then cooling to room temperature, wherein the heating rate during the heating process is 0.1°C / min, and the cooling rate during the cooling process is 0.1°C / min;

[0028] After the solvothermal reaction was completed, the solution in the reactor was filtered, and then washed three times with a mixed detergent of acetonitrile and deionized water in a volume ratio of 1:1, and then vacuum dried to obtain light blue block crystals, which were copper (II) catalysts with a molecular formula of C 18 H 14 CuN3O6, yield is 72.3%.

[0029] The chemical structural formula of the 3-PDCA ligand used in this embodiment is:

[0030] The chemical structure of 4,4'-bipyridine is:

[0031] 3-PDCA ligand and 4,4'-bipyridine are bridging organic acid ligands, which function to connect adjacent metal nodes; they have good chemical stability and reactivity, and can obtain a stable coordination polymer with catalytic performance.

[0032] In this embodiment, one copper ion is coordinated with the 3-PDCA ligand and the 4,4'-bipyridine ligand at the same time, and two bridging ligands are used to form a special hexagonal network structure, thereby obtaining a copper (II) catalyst with a novel structure.

[0033] The catalytic performance test of vinyl chloride found that the copper (II) catalyst has good stability and can be used as a catalyst in the process of synthesizing vinyl chloride from hydrogen chloride and acetylene.

[0034] Example 2

[0035] S1. Take 0.05 mmol of 3-PDCA ligand and 0.05 mmol of 4,4'-bipyridine ligand and add them to 2 mL of acetonitrile, and stir them evenly at a speed of 1200 rpm to obtain an acetonitrile suspension;

[0036] S2, take 0.1mmol of copper nitrate trihydrate and dissolve it in 3mL of deionized water, stir it evenly at a speed of 1200rpm to obtain a copper nitrate trihydrate solution;

[0037] S3, adding the copper nitrate trihydrate solution prepared in S2 to the acetonitrile suspension prepared in S1, stirring at a rotation speed of 1200 rpm to obtain a mixed suspension, wherein the volume ratio of the copper nitrate trihydrate solution to the acetonitrile suspension is 1:1, placing the mixed suspension in a high-pressure reactor, and performing a solvothermal reaction under programmed temperature control, wherein the specific temperature control program is: heating to 110°C and maintaining for 72 hours, and then cooling to room temperature, wherein the heating rate during the heating process is 0.1°C / min, and the cooling rate during the cooling process is 0.1°C / min;

[0038] After the solvothermal reaction was completed, the solution in the reactor was filtered, and then washed three times with a mixed detergent of acetonitrile and deionized water in a volume ratio of 1:1, and then vacuum dried to obtain light blue block crystals, which were copper (II) catalysts with a molecular formula of C 18 H 14 CuN3O6, yield is 71.1%.

[0039] Example 3

[0040] This embodiment provides a method for preparing a copper (II) catalyst, comprising the following steps:

[0041] S1. Take 0.05 mmol of 3-PDCA ligand and 0.05 mmol of 4,4'-bipyridine ligand and add them to 4 mL of acetonitrile, and stir them evenly at a speed of 1200 rpm to obtain an acetonitrile suspension;

[0042] S2, take 0.1mmol of copper nitrate trihydrate and dissolve it in 3mL of deionized water, stir it evenly at a speed of 1200rpm to obtain a copper nitrate trihydrate solution;

[0043] S3, adding the copper nitrate trihydrate solution prepared in S2 to the acetonitrile suspension prepared in S1, stirring at a rotation speed of 1200 rpm to obtain a mixed suspension, wherein the volume ratio of the copper nitrate trihydrate solution to the acetonitrile suspension is 1:1, placing the mixed suspension in a high-pressure reactor, and performing a solvothermal reaction under programmed temperature control, wherein the specific temperature control program is: heating to 110°C and maintaining for 72 hours, and then cooling to room temperature, wherein the heating rate during the heating process is 0.1°C / min, and the cooling rate during the cooling process is 0.1°C / min;

[0044] After the solvothermal reaction was completed, the solution in the reactor was filtered, and then washed three times with a mixed detergent of acetonitrile and deionized water in a volume ratio of 1:1, and then vacuum dried to obtain light blue block crystals, which were copper (II) catalysts with a molecular formula of C 18 H 14 CuN3O6, yield is 70.6%.

[0045] Example 4

[0046] S1. Take 0.05 mmol of 3-PDCA ligand and 0.05 mmol of 4,4'-bipyridine ligand and add them to 3 mL of acetonitrile, and stir them evenly at a speed of 1200 rpm to obtain an acetonitrile suspension;

[0047] S2, take 0.1mmol of copper nitrate trihydrate and dissolve it in 1mL of deionized water, stir it evenly at a speed of 1200rpm to obtain a copper nitrate trihydrate solution;

[0048] S3, adding the copper nitrate trihydrate solution prepared in S2 to the acetonitrile suspension prepared in S1, stirring at a rotation speed of 1200 rpm to obtain a mixed suspension, wherein the volume ratio of the copper nitrate trihydrate solution to the acetonitrile suspension is 1:1, placing the mixed suspension in a high-pressure reactor, and performing a solvothermal reaction under programmed temperature control, wherein the specific temperature control program is: heating to 110°C and maintaining for 72 hours, and then cooling to room temperature, wherein the heating rate during the heating process is 0.1°C / min, and the cooling rate during the cooling process is 0.1°C / min;

[0049] After the solvothermal reaction was completed, the solution in the reactor was filtered, and then washed three times with a mixed detergent of acetonitrile and deionized water in a volume ratio of 1:1, and then vacuum dried to obtain light blue block crystals, which were copper (II) catalysts with a molecular formula of C 18 H 14 CuN3O6, yield is 69.7%.

[0050] Comparative Example 1

[0051] Compared with Example 1, this comparative example cancels the solvent thermal reaction in S3 and evaporates slowly at room temperature. The specific operation is as follows:

[0052] S1. Take 0.05 mmol of 3-PDCA ligand and 0.05 mmol of 4,4'-bipyridine ligand and add them to 3 mL of acetonitrile, and stir them evenly at a speed of 1200 rpm to obtain an acetonitrile suspension;

[0053] S2, take 0.1mmol of copper nitrate trihydrate and dissolve it in 3mL of deionized water, stir it evenly at a speed of 1200rpm to obtain a copper nitrate trihydrate solution;

[0054] S3. Add the copper nitrate trihydrate solution prepared in S2 to the acetonitrile suspension prepared in S1, and stir evenly at a rotation speed of 1200 rpm to obtain a mixed suspension, wherein the volume ratio of the copper nitrate trihydrate solution to the acetonitrile suspension is 1:1, place the mixed suspension in a container, seal the container with plastic wrap and pierce small holes in the plastic wrap, place the sealed and pierced container in a room temperature environment, and after slow evaporation, no testable crystals are finally obtained.

[0055] Comparative Example 2

[0056] In this comparative example, compared with Example 1, the washed product is directly evaporated at room temperature without vacuum drying. The specific steps are as follows:

[0057] S1. Take 0.05 mmol of 3-PDCA ligand and 0.05 mmol of 4,4'-bipyridine ligand and add them to 3 mL of acetonitrile, and stir them evenly at a speed of 1200 rpm to obtain an acetonitrile suspension;

[0058] S2, take 0.1mmol of copper nitrate trihydrate and dissolve it in 3mL of deionized water, stir it evenly at a speed of 1200rpm to obtain a copper nitrate trihydrate solution;

[0059] S3, adding the copper nitrate trihydrate solution prepared in S2 to the acetonitrile suspension prepared in S1, stirring at a rotation speed of 1200 rpm to obtain a mixed suspension, wherein the volume ratio of the copper nitrate trihydrate solution to the acetonitrile suspension is 1:1, placing the mixed suspension in a high-pressure reactor, and performing a solvothermal reaction under programmed temperature control, wherein the specific temperature control program is: heating to 110°C and maintaining for 72 hours, and then cooling to room temperature, wherein the heating rate during the heating process is 0.1°C / min, and the cooling rate during the cooling process is 0.1°C / min;

[0060] The solution in the reactor was then filtered, and then washed three times with a mixed detergent of acetonitrile and deionized water in a volume ratio of 1:1. The washed product was then placed in a container, sealed with plastic wrap and small holes were pierced in the plastic wrap, and the sealed and pierced container was placed in a room temperature environment to allow the remaining solvent to evaporate slowly, and finally a powdered solid was obtained.

[0061] Comparative Example 3

[0062] In this comparative example, relative to Example 1, the temperature control procedure of the solvent thermal reaction is modified, and the specific steps are as follows:

[0063] S1. Take 0.05 mmol of 3-PDCA ligand and 0.05 mmol of 4,4'-bipyridine ligand and add them to 3 mL of acetonitrile, and stir them evenly at a speed of 1200 rpm to obtain an acetonitrile suspension;

[0064] S2, take 0.1mmol of copper nitrate trihydrate and dissolve it in 3mL of deionized water, stir it evenly at a speed of 1200rpm to obtain a copper nitrate trihydrate solution;

[0065] S3, adding the copper nitrate trihydrate solution prepared in S2 to the acetonitrile suspension prepared in S1, stirring at a rotation speed of 1200 rpm to obtain a mixed suspension, wherein the volume ratio of the copper nitrate trihydrate solution to the acetonitrile suspension is 1:1, placing the mixed suspension in a high-pressure reactor, and performing a solvothermal reaction under programmed temperature control, wherein the specific temperature control program is: heating to 90°C and maintaining for 72 hours, and then cooling to room temperature, wherein the heating rate during the heating process is 0.1°C / min, and the cooling rate during the cooling process is 0.1°C / min;

[0066] The solution in the reactor was then filtered, washed three times with acetonitrile and deionized water in a volume ratio of 1:1, and then vacuum dried to obtain light blue block crystals.

[0067] Example 5

[0068] The elemental analysis of the blue block crystals finally obtained in Example 1 showed that: 18 H 14 CuN3O6, molecular weight 431.86.

[0069] The blue block crystals finally obtained in Example 1 were tested using a Bruker SMART 1000CCD surface diffractometer, with a specific wavelength of MoKα rays, ω scanning mode. The collected diffraction points were restored using the SAINT program, and the data were corrected using the SADABS program. Based on the full-angle least squares method, the crystal solution software SHELXTL 5.1 package was used to find the coordinates of all non-hydrogen atoms on the difference Fourier map using the direct method, and then all non-hydrogen atoms were refined anisotropically. The schematic diagram of the solved molecular structure is shown in Figure 1 The obtained crystallographic parameters are shown in Table 1:

[0070] Table 1

[0071]

[0072]

[0073] R1=∑||F o |-|F c || / ∑|F o |,wR2=[∑w(F o 2 -F c 2 ) 2 / ∑w(F o 2 ) 2 ] 1 / 2 .

[0074] As can be seen from Table 1, the R1 value is less than 0.05, indicating that there is no error in the structural analysis and the true molecular structure is obtained.

[0075] Example 6

[0076] In this example, the catalyst activity of the blue block crystals finally obtained in Example 1 was evaluated.

[0077] Take 50 mg of the blue block crystals obtained in Example 1 and load them into a stainless steel fixed bed reactor with an inner diameter of 25 mm. The reactor is temperature-controlled by a thermocouple. The hydrogen chloride and acetylene are purified and dried and then enter the premixing device. V(HCI): V(C2H2) = 1.05, and the air velocity is 90 h -1 The tail gas after the reaction is washed with sodium hydroxide solution, deacidified and dried before entering the gas chromatograph, and the catalytic performance of the catalyst is detected by gas chromatography analysis.

[0078] This embodiment uses a GC-9790 gas chromatograph, a GDX-301 packed column, and a FID detector, wherein the column temperature is 150° C., the detector temperature is 120° C., the analyzed components are acetylene, vinyl chloride, and ethylene dichloride, and the external standard method is used to measure the amount fraction of each component.

[0079] The catalytic performance of the blue block crystals obtained in Example 1 as a catalyst is evaluated by the acetylene conversion rate (X) and vinyl chloride selectivity (S). Since hydrogen chloride is absorbed and removed after the reaction, the entire reaction system can be regarded as unchanged in the calculation, and the total volume is calculated according to 1 volume unit. The calculation formula is:

[0080]

[0081] In the formula, is the residual acetylene volume fraction; is the volume fraction of vinyl chloride.

[0082] The acetylene conversion rate and vinyl chloride selectivity curve obtained from the catalyst performance test are as follows: Figure 3 As shown by Figure 3 It can be seen that the copper (II) catalyst prepared in Example 1 has a higher acetylene conversion rate and vinyl chloride selectivity as a catalyst in the process of synthesizing vinyl chloride from hydrogen chloride and acetylene.

[0083] The copper (II) catalyst maintained an acetylene conversion rate of 96.3% and a vinyl chloride selectivity of 98.1% within 2400 hours. Compared with traditional catalysts, it has the advantages of good stability, high conversion rate and high selectivity.

[0084] It can be seen from the above experimental results that the copper (II) catalyst in the present invention has a higher acetylene conversion rate and better stability. More importantly, the development of new coordination polymer catalysts to replace traditional catalysts becomes possible, which can fill the industry gap in the mercury-free production of polyvinyl chloride by the calcium carbide process.

[0085] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A copper (II) catalyst, characterized in that The molecular formula of the copper (II) catalyst is C 18 H 14 CuN3O6.

2. A method for preparing a copper (II) catalyst as claimed in claim 1, characterized in that: The following steps are involved: S1. Add 3-PDCA ligand and 4,4'-bipyridine ligand into acetonitrile and stir evenly to obtain acetonitrile suspension; S2, dissolving copper nitrate trihydrate in deionized water and stirring evenly to obtain a copper nitrate trihydrate solution; S3. Add the copper nitrate trihydrate solution prepared in S2 to the acetonitrile suspension prepared in S1, stir evenly, and after solvent thermal reaction, filter, wash and vacuum dry in sequence to obtain a copper (II) catalyst.

3. The preparation method according to claim 2, characterized in that: The molar volume ratio of the 3-PDCA ligand, 4,4'-bipyridine ligand and acetonitrile in S1 is 0.05 mmol: 0.05 mmol: 2-4 mL.

4. The preparation method according to claim 2, characterized in that: The molar volume ratio of copper nitrate trihydrate and deionized water in S2 is 0.1 mmol: 1-3 mL.

5. The preparation method according to claim 2, characterized in that: The temperature control procedure of the solvothermal reaction in S3 is: heating to 110°C and maintaining for 48 hours, then cooling to room temperature, the heating rate of the heating is 0.1°C / min, and the cooling rate of the cooling is 0.1°C / min.

6. The preparation method according to claim 2, characterized in that: The volume ratio of the hydrated copper nitrate solution and the acetonitrile suspension in S3 is 1:

1.

7. The preparation method according to claim 2, characterized in that: The detergent used for washing in S3 is a mixed detergent of acetonitrile and deionized water, and the volume ratio of acetonitrile to deionized water in the mixed detergent is 1:

1.

8. The preparation method according to claim 2, characterized in that: The stirring speed in S1, S2 and S3 is 1200 rpm.

9. Use of a copper (II) catalyst as claimed in any one of claims 1 to 8, characterized in that: The copper (II) catalyst is used for catalyzing the synthesis of polyvinyl chloride.

Citation Information

Patent Citations

  • Copper-based catalyst for preparing vinyl chloride through acetylene hydrochlorination reaction as well as preparation method and application of copper-based catalyst

    CN115779968A

  • Acetylene copper hydrochloride complex catalyst as well as preparation method and application thereof

    CN117772289A

  • Preparation method and application of binuclear complex of silver