Preparation method of sodium alginate hydrogel film containing nitrogen-doped carbon dots
By covalently crosslinking with nitrogen-doped carbon dots in sodium alginate hydrogel, a sodium alginate hydrogel film with excellent antioxidant and antibacterial properties was prepared, and the sodium alginate water in the prior art was solved The problem of insufficient antibacterial and antioxidant properties of the gel membrane achieves the improvement of the mechanical and swelling properties of the membrane, and significantly inhibits microbial growth in the storage of cooled meat.
Patent Information
- Application Number
- CN202310529968.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, sodium alginate hydrogel film has insufficient antibacterial and antioxidant properties, and there is little research on carbon dots in active hydrogel films, and there is a lot of room for improvement in performance, especially in mechanical properties and There is room for improvement in swelling performance.
By covalently crosslinking nitrogen-doped carbon dots with sodium alginate hydrogel under specific conditions, a nitrogen-doped carbon dots sodium alginate hydrogel film with outstanding antioxidant and antibacterial properties was prepared. The rich surface functional groups of the carbon dots are crosslinked with sodium alginate to form a film with excellent mechanical properties and swelling properties.
The prepared membrane exhibits significant antioxidant, antibacterial, improved water absorption rate and gel strength, while maintaining good biodegradability and green environmental protection characteristics, which can effectively inhibit the growth of microorganisms in the cooling meat and delay the cooling meat. The sensory quality is reduced.
Smart Images

Figure BDA0004224268590000041
Abstract
Description
Technical Field
[0001] The invention provides a method for preparing a sodium alginate hydrogel film containing nitrogen-doped carbon dots with antibacterial and antioxidant properties, in particular to a sodium alginate / nitrogen-doped carbon dot active hydrogel film, belonging to the field of natural polymer materials. Background Art
[0002] Sodium alginate hydrogel film is a three-dimensional network formed by cross-linking sodium alginate that can accommodate water molecules. It has the properties of both solid and liquid and can swell but cannot dissolve. 2+ Cross-linking is a common cross-linking method, but it requires CaCO3 solid to participate in the reaction in a weak acid environment to form a sodium alginate hydrogel film with uniform structure and performance. In recent years, active sodium alginate hydrogel films with antibacterial and antioxidant properties have been widely studied and have shown unique advantages in the fields of medical care, bioengineering and food preservation.
[0003] Carbon dots are a new type of fluorescent carbon-based nanomaterials with a size less than 10 nm. Due to their low toxicity, good biocompatibility, and excellent antibacterial and antioxidant properties, they have good development prospects in analytical detection, bioimaging, photocatalysis, LED luminescence, anti-counterfeiting encryption, etc. However, there are relatively few studies on their use in active hydrogel films. At the same time, surface functionalization and heteroatom doping techniques can effectively improve the performance of CDs and expand their application range. Nitrogen doping, as the most common doping method, has been proven to change the chemical structure of CDs, providing CDs with abundant functional groups and active sites, further improving their performance.
[0004] The abundant surface functional groups on the carbon dots can be cross-linked with the hydrogel through covalent bonds or non-covalent bonds to become a matrix for accommodating fluorescent CDs. According to the source of the hydrogel, the sodium alginate hydrogel is endowed with excellent antioxidant and antibacterial properties. The present invention uses sodium alginate as the hydrogel film matrix, and covalently cross-links with plasticizers, nitrogen-doped carbon dots, etc. under certain conditions to prepare a sodium alginate hydrogel film with outstanding antioxidant and antibacterial properties, as well as good mechanical properties and swelling properties. The hydrogel film is a green organic polymer material with development prospects. Summary of the invention
[0005] The purpose of the present invention is to provide a nitrogen-doped carbon dot sodium alginate hydrogel film with excellent antibacterial and antioxidant properties and a preparation method thereof in view of the above-mentioned problems and shortcomings. In order to achieve the above-mentioned purpose, the technical solution of the present invention is:
[0006] A nitrogen-doped carbon dot sodium alginate hydrogel film and a preparation method thereof, comprising the following steps:
[0007] (1) Add citric acid and urea into distilled water, stir until completely dissolved, then heat with a microwave, cool to room temperature, and take out the reaction product to obtain a crude carbon dot product.
[0008] (2) The solid obtained in step (1) was dispersed by ultrasonic until it was completely dissolved, the suspended solid was centrifuged, and the supernatant was filtered with a 0.45 μm filter membrane. Finally, the powdered CDs were collected by freeze drying and stored at 4° C. for future use.
[0009] (3) Dispersing a certain amount of calcium carbonate in distilled water to obtain a calcium carbonate dispersion for later use. Then adding a certain amount of sodium alginate powder into the distilled water, stirring until completely dissolved to obtain a uniform sodium alginate solution, and adding glycerol in the same proportion as the sodium alginate as a plasticizer.
[0010] (4) adding CDs solutions prepared with different contents to the nitrogen-doped carbon dot sodium alginate solution prepared in step (3), and stirring at room temperature until the mixture is uniform;
[0011] (5) After ultrasonic degassing treatment, the film-forming solution obtained in (4) is poured into a square plate (13×13 cm), and placed in a constant temperature blower dryer at 30° C. and 40% relative humidity for 7 h. After cooling to room temperature, the film is peeled off the plate and stored at 50% relative humidity and 24±1° C. for 24 h to obtain a finished product.
[0012] The beneficial effects of the present invention are:
[0013] (1) The present invention uses biodegradable sodium alginate and carbon dots with biocompatibility, antibacterial and antioxidant properties as raw materials. The prepared film has improved antioxidant and antibacterial properties, water absorption rate, and gel strength, and has no effect on swelling properties. It is biodegradable and environmentally friendly.
[0014] (2) The present invention provides an antibacterial and antioxidant nitrogen-doped carbon dot sodium alginate hydrogel film and a preparation method thereof. The operation process for preparing the hydrogel film is simple, the prepared film has uniform thickness, uniform color, no special odor, and has good biodegradability, antibacterial and antioxidant properties. The antibacterial and antioxidant properties of carbon dots are utilized to add them to the film instead of directly adding them to food to prepare an antibacterial and antioxidant active packaging film. At the same time, the carbon dot solution is acidic, which can precipitate calcium ions in calcium carbonate and form hydrogen bonds with the carboxyl groups of sodium alginate, thereby forming crosslinks.
[0015] (3) The membrane of the present invention absorbs the exudate of the chilled meat during storage, reducing the nutrients provided by the exudate to the microorganisms in the chilled meat, thereby inhibiting the growth and reproduction of the microorganisms in the chilled meat and slowing down the decline in the sensory quality of the chilled meat. DETAILED DESCRIPTION
[0016] The specific embodiments of the present invention are described in detail below:
[0017] A nitrogen-doped carbon dot sodium alginate hydrogel film and a preparation method thereof, comprising the following steps:
[0018] (1) Preparation of carbon dots: 0.5 g of citric acid and 0.5 g of urea were added to 5 mL of distilled water and stirred until completely dissolved. The mixture was then heated in a microwave at 700 W for 180 s. After cooling to room temperature, the reaction product was taken out to obtain a crude carbon dot product.
[0019] (2) The solid obtained in step (1) was dispersed by ultrasonic until it was completely dissolved, the suspended solid was centrifuged, and the supernatant was filtered with a 0.45 μm filter membrane. Finally, the powdered CDs were collected by freeze drying and stored at 4° C. for future use.
[0020] (3) Preparation of sodium alginate solution: 0.25 g of calcium carbonate was dispersed in 100 mL of distilled water to obtain a 0.25% (w / v) calcium carbonate dispersion for later use. Then 2 g of sodium alginate powder was added to 100 mL of distilled water and stirred until completely dissolved to obtain a uniform sodium alginate solution, and glycerol was added in the same proportion as the sodium alginate as a plasticizer.
[0021] (4) adding different mass CDs solutions (5%, 15%, 30%) to the nitrogen-doped carbon dot sodium alginate solution prepared in step (3), and stirring at room temperature until the mixture is uniform;
[0022] (5) After ultrasonic degassing treatment, the film-forming solution obtained in (4) is poured into a square plate (13×13 cm), and placed in a constant temperature blower dryer at 30° C. and 40% relative humidity for 7 h. After cooling to room temperature, the film is peeled off the plate and stored at 50% relative humidity and 24±1° C. for 24 h to obtain a finished product.
[0023] Example 1: A nitrogen-doped carbon dot sodium alginate hydrogel film and a preparation method thereof, comprising the following steps:
[0024] (1) Preparation of carbon dots: 0.5 g of citric acid and 0.5 g of urea were added to 5 mL of distilled water and stirred until completely dissolved. The mixture was then heated in a microwave at 700 W for 180 s. After cooling to room temperature, the reaction product was taken out to obtain a crude carbon dot product.
[0025] (2) The solid obtained in step (1) was dispersed by ultrasonic until it was completely dissolved, the suspended solid was centrifuged, and the supernatant was filtered with a 0.45 μm filter membrane. Finally, the powdered CDs were collected by freeze drying and stored at 4° C. for future use.
[0026] (3) Preparation of sodium alginate solution: 0.25 g of calcium carbonate was dispersed in 100 mL of distilled water to obtain a 0.25% (w / v) calcium carbonate dispersion for later use. Then 2 g of sodium alginate powder was added to 100 mL of distilled water and stirred until completely dissolved to obtain a uniform sodium alginate solution, and glycerol was added in the same proportion as the sodium alginate as a plasticizer.
[0027] (4) preparing CDs powder to a concentration of 5%, adding it to the nitrogen-doped carbon dot sodium alginate solution obtained in step (3), and stirring at room temperature until the mixture is uniformly mixed;
[0028] (5) After ultrasonic degassing treatment, the film-forming solution obtained in (4) is poured into a square plate (13×13 cm), and placed in a constant temperature blower dryer at 30° C. and 40% relative humidity for 7 h. After cooling to room temperature, the film is peeled off the plate and stored at 50% relative humidity and 24±1° C. for 24 h to obtain a finished product.
[0029] Example 2: A nitrogen-doped carbon dot sodium alginate hydrogel film and a preparation method thereof, comprising the following steps:
[0030] (1) Preparation of carbon dots: 0.5 g of citric acid and 0.5 g of urea were added to 5 mL of distilled water and stirred until completely dissolved. The mixture was then heated in a microwave at 700 W for 180 s. After cooling to room temperature, the reaction product was taken out to obtain a crude carbon dot product.
[0031] (2) The solid obtained in step (1) was dispersed by ultrasonic until it was completely dissolved, the suspended solid was centrifuged, and the supernatant was filtered with a 0.45 μm filter membrane. Finally, the powdered CDs were collected by freeze drying and stored at 4° C. for future use.
[0032] (3) Preparation of sodium alginate solution: 0.25 g of calcium carbonate was dispersed in 100 mL of distilled water to obtain a 0.25% (w / v) calcium carbonate dispersion for later use. Then 2 g of sodium alginate powder was added to 100 mL of distilled water and stirred until completely dissolved to obtain a uniform sodium alginate solution, and glycerol was added in the same proportion as the sodium alginate as a plasticizer.
[0033] (4) preparing CDs powder to a concentration of 15%, adding it to the nitrogen-doped carbon dot sodium alginate solution obtained in step (3), and stirring at room temperature until the mixture is uniformly mixed;
[0034] (5) After ultrasonic degassing treatment, the film-forming solution obtained in (4) is poured into a square plate (13×13 cm), and placed in a constant temperature blower dryer at 30° C. and 40% relative humidity for 7 h. After cooling to room temperature, the film is peeled off the plate and stored at 50% relative humidity and 24±1° C. for 24 h to obtain a finished product.
[0035] Example 3: A nitrogen-doped carbon dot sodium alginate hydrogel film and a preparation method thereof, comprising the following steps:
[0036] (1) Preparation of carbon dots: 0.5 g of citric acid and 0.5 g of urea were added to 5 mL of distilled water and stirred until completely dissolved. The mixture was then heated in a microwave at 700 W for 180 s. After cooling to room temperature, the reaction product was taken out to obtain a crude carbon dot product.
[0037] (2) The solid obtained in step (1) was dispersed by ultrasonic until it was completely dissolved, the suspended solid was centrifuged, and the supernatant was filtered with a 0.45 μm filter membrane. Finally, the powdered CDs were collected by freeze drying and stored at 4° C. for future use.
[0038] (3) Preparation of sodium alginate solution: 0.25 g of calcium carbonate was dispersed in 100 mL of distilled water to obtain a 0.25% (w / v) calcium carbonate dispersion for later use. Then 2 g of sodium alginate powder was added to 100 mL of distilled water and stirred until completely dissolved to obtain a uniform sodium alginate solution, and glycerol was added in the same proportion as the sodium alginate as a plasticizer.
[0039] (4) preparing CDs powder to a concentration of 30%, adding it to the nitrogen-doped carbon dot sodium alginate solution obtained in step (3), and stirring at room temperature until the mixture is uniformly mixed;
[0040] (5) After ultrasonic degassing treatment, the film-forming solution obtained in (4) is poured into a square plate (13×13 cm), and placed in a constant temperature blower dryer at 30° C. and 40% relative humidity for 7 h. After cooling to room temperature, the film is peeled off the plate and stored at 50% relative humidity and 24±1° C. for 24 h to obtain a finished product.
[0041] Control group 1: A pure sodium alginate hydrogel and a preparation method thereof, comprising the following steps:
[0042] (1) Preparation of sodium alginate solution: 0.25 g of calcium carbonate was dissolved in 100 mL of distilled water at room temperature to obtain a 0.25% (w / v) calcium carbonate solution for later use. Then, 2 g of sodium alginate powder was added to 100 mL of distilled water at 25°C and stirred until completely dissolved to obtain a uniform solution containing 2% (w / v) sodium alginate. Glycerol was used as a plasticizer in the same proportion as sodium alginate.
[0043] (2) Degassing and drying: The film-forming solution obtained in (1) was subjected to ultrasonic degassing for 15 min, poured into a square plate (13×13 cm), and placed in a constant temperature air drying machine at 30° C. and a relative humidity of 40% for drying for 7 h;
[0044] (3) Softening and peeling off the film: After cooling to room temperature, the film was peeled off from the plate and stored at 50% relative humidity and 24±1°C for 24 h;
[0045] (4) Finished product.
[0046] The nitrogen-doped carbon dot sodium alginate hydrogel films prepared in Examples 1-3 and the pure sodium alginate hydrogel prepared in Control Group 1 were tested for bacterial inhibition rate, DPPH free radical scavenging rate, ABTS free radical scavenging rate, water absorption rate, gel strength, and swelling rate;
[0047] The comparison results of the nitrogen-doped carbon dot sodium alginate hydrogel films prepared in Examples 1-3 and the pure sodium alginate hydrogel prepared in Control Group 1 are shown in the following table:
[0048]
[0049] Note: ① Each group of experiments was conducted in three parallel tests, and each value is the average of the three groups of data; ② DPPH free radical scavenging rate and ABTS free radical scavenging rate reflect the antioxidant property of the film. The higher the value, the higher the antioxidant property of the film; ③ Bacterial inhibition rate reflects the antibacterial property of the film. The higher the value, the higher the antibacterial property of the film; ④ Water absorption rate reflects the speed at which the film absorbs water. The lower the value, the slower the water absorption speed of the film; ⑤ Gel strength reflects the gel performance of the film. The higher the value, the better the gel performance of the film; ⑥ Swelling rate reflects the water absorption performance of the film. The higher the value, the better the water absorption performance of the film.
Claims
1. A method for preparing a nitrogen-doped carbon dot sodium alginate hydrogel film, characterized in that: The following steps are involved: (1) Add citric acid and urea into distilled water, stir until completely dissolved, then heat with a microwave, cool to room temperature, and take out the reaction product to obtain a crude carbon dot product. (2) The solid obtained in step (1) was dispersed by ultrasonic until it was completely dissolved, the suspended solid was centrifuged, and the supernatant was filtered with a 0.45 μm filter membrane. Finally, the powdered CDs were collected by freeze drying and stored at 4° C. for future use. (3) Dispersing a certain amount of calcium carbonate in distilled water to obtain a calcium carbonate dispersion for later use. Then adding a certain amount of sodium alginate powder into the distilled water, stirring until completely dissolved to obtain a uniform sodium alginate solution, and adding glycerol in the same proportion as the sodium alginate as a plasticizer. (4) adding the prepared CDs solutions of different concentrations to the nitrogen-doped carbon dot sodium alginate solution prepared in step (3), and stirring at room temperature until the mixture is uniform; (5) After ultrasonic degassing treatment, the film-forming solution obtained in (4) is poured into a square plate (13×13 cm), and placed in a constant temperature blower dryer at 30° C. and 40% relative humidity for 7 h. After cooling to room temperature, the film is peeled off the plate and stored at 50% relative humidity and 24±1° C. for 24 h to obtain a finished product.
2. The method for preparing a nitrogen-doped carbon dot sodium alginate hydrogel film according to claim 1, characterized in that The mass ratio of citric acid to urea in step (1) is 1:1, and the microwave conditions are controlled as follows: wattage 700w, time 180s.
3. The method for preparing a nitrogen-doped carbon dot sodium alginate hydrogel film according to claim 1, characterized in that In step (2), the amount of distilled water added is 20 mL, and the suspension centrifugation conditions are controlled as follows: the number of revolutions is 5000 rpm, and the time is 15 min. The freeze-drying conditions are pre-freezing for 24 hours and freeze-drying for 48 hours.
4. The method for preparing a nitrogen-doped carbon dot sodium alginate hydrogel film according to claim 1, characterized in that In the step (3), the concentration of sodium alginate is 2%, and the concentration of calcium carbonate is 0.25%.
5. The method for preparing a nitrogen-doped carbon dot sodium alginate hydrogel film according to claim 1, characterized in that In the step (4), carbon dot solutions with concentrations of 5%, 15%, and 30% (w / v) are added.
6. The method for preparing a nitrogen-doped carbon dot sodium alginate hydrogel film according to claim 1, characterized in that In the step (5), the ultrasonic degassing treatment time is 15 minutes, and the drying conditions are controlled as follows: temperature 30° C., relative humidity 40%, and time 7 hours.
Citation Information
Cited By
Zinc-doped antibacterial carbon dots as well as preparation method and application thereof
CN119499279A
Submerged plant root system growth promoting substrate and application thereof
CN120188697A
Double-carbon-dot food antibacterial and visual monitoring intelligent packaging material as well as preparation method and application thereof