Method for dissolving cellulose by ionic liquid under mild condition and preparing regenerated cellulose fiber or film

By using phosphite ionic liquids to dissolve cellulose under mild conditions and using dry spray-wet method or casting method to prepare regenerated cellulose materials, the problems of high temperature and high energy consumption and pollution in the prior art are solved, and high efficiency is achieved. Environmentally friendly cellulose material production with excellent mechanical properties and sustainability.

CN118930916APending Publication Date: 2024-11-12INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES +1

Patent Information

Application Number
CN202411063613.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing cellulose solvent system has problems such as high temperature, high energy consumption, pollution and complex processes, and it is difficult to efficiently dissolve cellulose under mild conditions, which limits the green and low-carbon industrial production of regenerated cellulose materials.

Method used

The phosphite ionic liquid and cellulose are mixed with the ionic liquid and dissolved under mild conditions to obtain a transparent and uniform ionic liquid-cellulose solution. The regenerated cellulose fibers are prepared by dry spray-wet spinning or casting method or Thin film and ionic liquid can be recycled and reused.

Benefits of technology

It realizes efficient dissolution of cellulose under mild conditions, simplifies processes, reduces energy consumption, improves the mechanical properties of cellulose materials, and meets environmentally friendly and sustainable development requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for dissolving cellulose by ionic liquid under mild conditions and preparing regenerated cellulose fibers or films. The method comprises the following steps: (1) adding washed and dried cellulose and a phosphite ionic liquid aqueous solution into a reaction kettle according to a certain proportion, and swelling at room temperature; (2) defoaming and dissolving at a certain temperature, filtering the obtained ionic liquid-cellulose solution, and preparing regenerated cellulose fibers by adopting a dry spraying-wet spinning process, or preparing a regenerated cellulose film by adopting a tape casting method; and (3) recycling the ionic liquid in the coagulating bath. The method is simple in process, mild in cellulose dissolving condition and environment-friendly, and the prepared regenerated cellulose fibers and films have excellent mechanical properties. A novel mild dissolution method is provided for a process for preparing cellulose fibers or films by dissolving cellulose with ionic liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing regenerated cellulose fiber and a regenerated cellulose film, and in particular to a method for dissolving cellulose in an ionic liquid under mild conditions and preparing the regenerated cellulose fiber or film. Technical Background

[0002] Cellulose is the most abundant biopolymer in nature and can be continuously replenished through plant growth. Due to its low cost, renewability, excellent biocompatibility and biodegradability, cellulose has become an ideal candidate material to replace traditional plastics and chemical materials. Cellulose has shown great application potential in many fields such as textiles, packaging and biomedicine. Among them, regenerated cellulose fibers have been widely used in the textile industry due to their controllability, versatility and high performance. However, the highly ordered structure and complex hydrogen bond network of natural cellulose make it difficult to dissolve, which poses a huge challenge to the manufacture of regenerated cellulose materials. In order to improve the solubility of cellulose in solvents, researchers have adopted a variety of methods such as steam explosion, alkalization, hydrothermal and enzyme treatment, but these methods often lead to partial degradation of cellulose chains. Although the traditional sodium hydroxide / carbon disulfide solvent has been used for many years, it is in urgent need of more environmentally friendly alternative solvents due to its high pollution and high energy consumption. The commonly used solvent systems currently include lithium chloride (LiCl) / dimethylacetamide (DMAc) and N-methylmorpholine-N-oxide (NMMO) / water. Although NMMO has been widely used in the Lyocell process, it still has problems such as poor thermal stability and high temperature explosion. To solve the problem of efficient conversion and utilization of cellulose, researchers are exploring more stable and environmentally friendly solvent systems to improve the feasibility and environmental friendliness of cellulose processing.

[0003] In recent years, ionic liquids have become the most promising green solvents in the cellulose industry due to their excellent solubility, chemical stability, recyclability and adjustability. The emergence of ionic liquids provides new possibilities for the efficient conversion and utilization of cellulose, shows great potential in the preparation of cellulose fibers or films, and provides new solutions for the sustainable development of the cellulose materials industry. Patents CN105801884A and CN1059949482A use 1-butyl-3-methylimidazolium chloride ionic liquid and 1-allyl-3-methylimidazolium chloride ionic liquid to dissolve cellulose, respectively, and add solid acid to improve the dissolution of the ionic liquid, reducing the degradation rate of cellulose. However, its dissolution temperature is still maintained at a relatively high temperature (80-120°C), and this chloride ionic liquid has a certain corrosiveness to metal equipment, which limits its promotion in the industrial application of regenerated cellulose materials. In addition, the patent (CN 109898169 A) also reported a method for dissolving cellulose with ionic liquids. Although this method appropriately reduces the dissolution temperature of cellulose, it requires acid and alkali pretreatment of natural cellulose, and the dissolution process requires shearing in an emulsifier, which has problems such as complex process and environmental pollution. Therefore, it is urgent to develop a new solvent system with simple process, mild conditions and green environmental protection to efficiently dissolve cellulose and further promote the green and low-carbon industrial production of cellulose materials. This paper uses phosphite ionic liquids to dissolve cellulose. Compared with the above-mentioned ionic liquids, this type of ionic liquid has milder dissolution conditions and has the potential for one-step synthesis and recyclable industrial conditions. It provides a green, environmentally friendly, low-carbon and energy-saving way for the efficient conversion and utilization of cellulose. Summary of the invention

[0004] The present invention provides a method for dissolving cellulose with ionic liquid under mild conditions and preparing regenerated cellulose fibers or films. The pretreated cellulose is mixed with a phosphite ionic liquid aqueous solution in a certain proportion, first swelled, and then stirred for degassing and dissolution under mild conditions. After the cellulose is completely dissolved, it is filtered to obtain a transparent and uniform ionic liquid-cellulose solution. Then, a dry-jet-wet spinning process is used to prepare regenerated cellulose fibers, or a casting method is used to prepare regenerated cellulose films. The method has mild cellulose dissolution conditions, a simple process, and is environmentally friendly. At the same time, the ionic liquid used can be recycled and reused, so that it has certain economic efficiency.

[0005] The technical solution of the present invention is a method for dissolving cellulose with an ionic liquid under mild conditions and preparing regenerated cellulose fibers or films, comprising the following steps:

[0006] (1) placing the washed and dried cellulose and a phosphite ionic liquid aqueous solution in a certain proportion into a reaction kettle and allowing them to swell at room temperature;

[0007] (2) stirring, degassing and dissolving cellulose at a certain temperature, filtering the obtained ionic liquid-cellulose solution, and preparing regenerated cellulose fibers by dry-jet-wet spinning process, or preparing regenerated cellulose film by casting method;

[0008] (3) Recycling the ionic liquid in the coagulation bath of step (2).

[0009] In the step (1), the ionic liquid is selected from any one or a combination of at least two of 1-R2-3-R1-imidazole phosphite methyl (or ethyl, or butyl) ester and 1-R2-1,5-diazabicyclo[4.3.0]-5-nonene phosphite methyl (or ethyl, or butyl) ester, wherein R1, R2 = C m H 2n+1 , m and n are values ​​ranging from 1 to 10, and are both positive integers.

[0010] The cellulose in step (1) may be one or more of microcrystalline cellulose, wood pulp cellulose, cotton pulp cellulose, mushroom grass cellulose, bamboo pulp cellulose, and paper pulp cellulose, and the degree of polymerization is between 220 and 2000.

[0011] In the step (1), the concentration of the ionic liquid aqueous solution used for swelling the cellulose is 40 to 80 wt%.

[0012] In the step (1), the mass ratio of cellulose to phosphite ionic liquid is (0.01-0.20):1, wherein the dissolution temperature is 40-80°C, the dissolution time is 3-8h, and the mechanical stirring speed is 100-300rpm.

[0013] The coagulation bath in step (2) can be one or more of water, methanol and ethanol.

[0014] In the step (2), the regenerated cellulose fiber has a breaking strength of 1.2 to 2.5 cN / dtex and an elongation of 8% to 13%, and the regenerated cellulose film has a tensile strength of 122.8 to 145.3 MPa and an elongation of 7.8 to 12.1%.

[0015] The beneficial effects of the present invention are:

[0016] (1) The present invention uses an ionic liquid aqueous solution to perform swelling treatment on cellulose, thereby improving the dissolution effect of cellulose.

[0017] (2) The present invention uses a novel phosphite ionic liquid to dissolve cellulose under mild conditions, and after filtration and degassing, a transparent, uniform, and stable ionic liquid-cellulose solution is obtained.

[0018] (3) The present invention adopts a dry-jet-wet spinning method to prepare regenerated cellulose fibers, or adopts a casting method to prepare regenerated cellulose films, which not only simplifies the process but also reduces energy consumption and avoids the damage of high temperature to the cellulose structure and polymerization degree.

[0019] (4) The regenerated cellulose fiber and film prepared by the present invention have excellent mechanical properties. In addition, the recycling and reuse of ionic liquids improves economic efficiency, meets the requirements of environmental friendliness and sustainable development, and has broad application prospects. Specific implementation methods

[0021] The present invention is further described in detail below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. The implementation conditions adopted in the embodiments can be further adjusted according to the different requirements of specific use. The following examples are only for explanation and should not be relied upon to limit the scope of protection of the present invention.

[0022] Embodiment 1:

[0023] (1) Washing and drying wood pulp cellulose (degree of polymerization 300), specifically comprising: washing the wood pulp cellulose with deionized water to remove impurities, and then drying at 60°C for 24 hours. Take 0.35g of the dried wood pulp cellulose, add 16.7g of 80% concentration of 1-methyl-3-methylimidazole methyl phosphite aqueous solution, swell at room temperature for 1 hour, and then degas and dissolve at a temperature of 50°C and a mechanical stirring speed of 180 rpm for 4.5 hours.

[0024] (2) After the dissolution is completed, the cellulose solution is filtered and regenerated cellulose fibers are prepared by a dry-jet wet spinning device, wherein the preparation process includes spinning, coagulation bath regeneration, water washing and drying, and then winding into a tube for storage. Alternatively, a cellulose film is prepared by a film casting method using a scraping machine, wherein the preparation process includes film casting, coagulation bath regeneration, water washing and drying.

[0025] Through testing, the breaking strength of the prepared regenerated cellulose fiber is 2.38 cN / dtex, and the elongation is 11.2%. The tensile strength of the regenerated cellulose film is 133.7 MPa, and the elongation is 10.3%.

[0026] (3) The ionic liquid in the coagulation bath is recovered and reused in step (1). The specific recovery step is as follows: the aqueous solution in the coagulation bath is filtered and flocculated and then distilled under reduced pressure at 80°C to recover the ionic liquid in the coagulation bath. The recovery rate of the ionic liquid is 96.8%. The regenerated cellulose fiber prepared by repeating steps (1) and (2) with the recovered ionic liquid has a breaking strength of 2.36 cN / dtex and an elongation of 11.1%. The regenerated cellulose film has a tensile strength of 131.2 MPa and an elongation of 10.1%.

[0027] Embodiment 2:

[0028] (1) Washing and drying wood pulp cellulose (degree of polymerization 500), specifically comprising: washing the wood pulp cellulose with deionized water to remove impurities, and then drying at 60° C. for 24 hours. Take 0.55 g of the dried wood pulp cellulose, add 18.5 g of a 60% concentration of 1-ethyl-3-methylimidazole methyl phosphite aqueous solution, swell at room temperature for 1 hour, and then degas and dissolve at a temperature of 60° C. and a mechanical stirring speed of 200 rpm for 4 hours.

[0029] (2) After the dissolution is completed, the cellulose solution is filtered and regenerated cellulose fibers are prepared by a dry-jet wet spinning device, wherein the preparation process includes spinning, coagulation bath regeneration, water washing and drying, and then winding into a tube for storage. Alternatively, a cellulose film is prepared by a film casting method using a scraping machine, wherein the preparation process includes film casting, coagulation bath regeneration, water washing and drying.

[0030] Through testing, the breaking strength of the prepared regenerated cellulose fiber is 1.97 cN / dtex, and the elongation is 10.2%. The tensile strength of the regenerated cellulose film is 136.6 MPa, and the elongation is 9.3%.

[0031] (3) The ionic liquid in the coagulation bath is recovered and reused in step (1). The specific recovery step is as follows: the aqueous solution in the coagulation bath is filtered and flocculated and precipitated, and then the ionic liquid in the coagulation bath is recovered by vacuum distillation at 80° C. The recovery rate of the ionic liquid is 96.4%. The regenerated cellulose fiber prepared by repeating steps (1) and (2) with the recovered ionic liquid has a breaking strength of 1.95 cN / dtex and an elongation of 10.3%. The regenerated cellulose film has a tensile strength of 136.2 MPa and an elongation of 9.1%.

[0032] Embodiment 3:

[0033] (1) Washing and drying wood pulp cellulose (degree of polymerization 640), specifically comprising: washing the wood pulp cellulose with deionized water to remove impurities, and then drying at 60°C for 24 hours. Take 0.45g of the dried wood pulp cellulose, add 16.5g of 80% 1-ethyl-3-methylimidazole ethyl phosphite aqueous solution, swell at room temperature for 1.5 hours, and then degas and dissolve at 70°C and 150rpm for 5 hours.

[0034] (2) After the dissolution is completed, the cellulose solution is filtered and regenerated cellulose fibers are prepared by a dry-jet wet spinning device, wherein the preparation process includes spinning, coagulation bath regeneration, water washing and drying, and then winding into a tube for storage. Alternatively, a cellulose film is prepared by a film casting method using a scraping machine, wherein the preparation process includes film casting, coagulation bath regeneration, water washing and drying.

[0035] Through testing, the breaking strength of the prepared regenerated cellulose fiber is 2.16 cN / dtex, and the elongation is 10.4%. The tensile strength of the regenerated cellulose film is 142.3 MPa, and the elongation is 8.7%.

[0036] (3) The ionic liquid in the coagulation bath is recovered and reused in step (1). The specific recovery step is as follows: the aqueous solution in the coagulation bath is filtered and flocculated and precipitated, and then the ionic liquid in the coagulation bath is recovered by vacuum distillation at 80° C. The recovery rate of the ionic liquid is 97.2%. The regenerated cellulose fiber prepared by repeating steps (1) and (2) with the recovered ionic liquid has a breaking strength of 2.14 cN / dtex and an elongation of 10.2%. The regenerated cellulose film has a tensile strength of 141.2 MPa and an elongation of 8.5%.

[0037] Embodiment 4:

[0038] (1) Washing and drying wood pulp cellulose (degree of polymerization 900), specifically comprising: washing the wood pulp cellulose with deionized water to remove impurities, and then drying at 60°C for 24 hours. Take 0.40g of the dried wood pulp cellulose, add 17.0g of 70% concentration of 1-ethyl-1,5-diazabicyclo[4.3.0]-5-nonene methyl phosphite, swell at room temperature for 1.5 hours, and then degas and dissolve at 70°C and 150 rpm for 4.5 hours.

[0039] (2) After the dissolution is completed, the cellulose solution is filtered and regenerated cellulose fibers are prepared by a dry-jet wet spinning device, wherein the preparation process includes spinning, coagulation bath regeneration, water washing and drying, and then winding into a tube for storage. Alternatively, a cellulose film is prepared by a film casting method using a scraping machine, wherein the preparation process includes film casting, coagulation bath regeneration, water washing and drying.

[0040] Through testing, the breaking strength of the prepared regenerated cellulose fiber is 2.28 cN / dtex, and the elongation is 10.8%. The tensile strength of the regenerated cellulose film is 127.6 MPa, and the elongation is 10.7%.

[0041] (3) The ionic liquid in the coagulation bath is recovered and reused in step (1). The specific recovery step is as follows: the aqueous solution in the coagulation bath is filtered and flocculated and precipitated, and then the ionic liquid in the coagulation bath is recovered by vacuum distillation at 80° C. The recovery rate of the ionic liquid is 97.0%. The regenerated cellulose fiber prepared by repeating steps (1) and (2) with the recovered ionic liquid has a breaking strength of 2.26 cN / dtex and an elongation of 10.7%. The regenerated cellulose film has a tensile strength of 124.8 MPa and an elongation of 9.7%.

[0042] Embodiment 5:

[0043] (1) Washing and drying wood pulp cellulose (degree of polymerization 640), specifically comprising: washing the wood pulp cellulose with deionized water to remove impurities, and then drying at 60°C for 24 hours. Take 0.7g of the dried wood pulp cellulose, add 18.0g of 80% 1-methyl-1,5-diazabicyclo[4.3.0]-5-nonene methyl phosphite aqueous solution, swell at room temperature for 1.5 hours, and then degas and dissolve at 70°C and 180 rpm for 5 hours.

[0044] (2) After the dissolution is completed, the cellulose solution is filtered and regenerated cellulose fibers are prepared by a dry-jet wet spinning device, wherein the preparation process includes spinning, coagulation bath regeneration, water washing and drying, and then winding into a tube for storage. Alternatively, a cellulose film is prepared by a film casting method using a scraping machine, wherein the preparation process includes film casting, coagulation bath regeneration, water washing and drying.

[0045] Through testing, the prepared regenerated cellulose fiber has a breaking strength of 1.86 cN / dtex and an elongation of 11.4%. The regenerated cellulose film has a tensile strength of 135.2 MPa and an elongation of 10.7%.

[0046] (3) The ionic liquid in the coagulation bath is recovered and reused in step (1). The specific recovery step is as follows: the aqueous solution in the coagulation bath is filtered and flocculated and then distilled under reduced pressure at 80° C. to recover the ionic liquid in the coagulation bath. The recovery rate of the ionic liquid is 96.2%. The regenerated cellulose fiber prepared by repeating steps (1) and (2) with the recovered ionic liquid has a breaking strength of 1.85 cN / dtex and an elongation of 11.2%. The regenerated cellulose film has a tensile strength of 133.6 MPa and an elongation of 10.5%.

[0047] Embodiment 6:

[0048] (1) Washing and drying wood pulp cellulose (degree of polymerization 640), specifically comprising: washing the wood pulp cellulose with deionized water to remove impurities, and then drying at 60°C for 24 hours. Take 0.4 g of the dried wood pulp cellulose, add 8.5 g of 80% aqueous solution of 1-butyl-3-methylimidazole methyl phosphite and 8.5 g of 80% aqueous solution of 1-methyl-3-methylimidazole methyl phosphite, swell at room temperature for 1 hour, and then degas and dissolve at 70°C and a mechanical stirring speed of 150 rpm for 4 hours.

[0049] (2) After the dissolution is completed, the cellulose solution is filtered and regenerated cellulose fibers are prepared by a dry-jet wet spinning device, wherein the preparation process includes spinning, coagulation bath regeneration, water washing and drying, and then winding into a tube for storage. Alternatively, a cellulose film is prepared by a film casting method using a scraping machine, wherein the preparation process includes film casting, coagulation bath regeneration, water washing and drying.

[0050] Through testing, the breaking strength of the prepared regenerated cellulose fiber is 2.30 cN / dtex, and the elongation is 9.7%. The tensile strength of the regenerated cellulose film is 144.2 MPa, and the elongation is 9.1%.

[0051] (3) The ionic liquid in the coagulation bath is recovered and reused in step (1). The specific recovery step is as follows: the aqueous solution in the coagulation bath is filtered and flocculated and then distilled under reduced pressure at 80°C to recover the ionic liquid in the coagulation bath. The recovery rate of the ionic liquid is 96.5%. The regenerated cellulose fiber prepared by repeating steps (1) and (2) with the recovered ionic liquid has a breaking strength of 2.28 cN / dtex and an elongation of 9.5%. The regenerated cellulose film has a tensile strength of 142.6 MPa and an elongation of 9.0%.

[0052] Embodiment 7:

[0053] (1) Washing and drying wood pulp cellulose (degree of polymerization 640), specifically comprising: washing the wood pulp cellulose with deionized water to remove impurities, and then drying at 60° C. for 24 h. Taking 0.6 g of the dried wood pulp cellulose, adding 18.5 g of 80% 1-butyl-3-methylimidazole ethyl phosphite aqueous solution, swelling at room temperature for 1 h, and then degassing and dissolving at 70° C. and a mechanical stirring speed of 150 rpm for 5.5 h.

[0054] (2) After the dissolution is completed, the cellulose solution is filtered and regenerated cellulose fibers are prepared by a dry-jet wet spinning device, wherein the preparation process includes spinning, coagulation bath regeneration, water washing and drying, and then winding into a tube for storage. Alternatively, a cellulose film is prepared by a film casting method using a scraping machine, wherein the preparation process includes film casting, coagulation bath regeneration, water washing and drying.

[0055] Through testing, the breaking strength of the prepared regenerated cellulose fiber is 1.96 cN / dtex, and the elongation is 11.2%. The tensile strength of the regenerated cellulose film is 132.7 MPa, and the elongation is 9.7%.

[0056] (3) The ionic liquid in the coagulation bath is recovered and reused in step (1). The specific recovery step is as follows: the aqueous solution in the coagulation bath is filtered and flocculated and precipitated, and then the ionic liquid in the coagulation bath is recovered by vacuum distillation at 80° C. The recovery rate of the ionic liquid is 97.0%. The regenerated cellulose fiber prepared by repeating steps (1) and (2) with the recovered ionic liquid has a breaking strength of 1.94 cN / dtex and an elongation of 11.0%. The regenerated cellulose film has a tensile strength of 132.4 MPa and an elongation of 9.5%.

[0057] The above embodiments are only part of the process methods of the present invention. Their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for dissolving cellulose with ionic liquid under mild conditions and preparing regenerated cellulose fibers or films. Characterized by: The following steps are involved: (1) placing the washed and dried cellulose and the ionic liquid aqueous solution in a certain ratio into a reaction kettle and allowing them to swell at room temperature; (2) stirring, degassing and dissolving cellulose at a certain temperature, filtering the obtained ionic liquid-cellulose solution, and preparing regenerated cellulose fibers by dry-jet-wet spinning process, or preparing regenerated cellulose film by casting method; (3) Recycling the ionic liquid in the coagulation bath of step (2).

2. The method for dissolving cellulose with ionic liquid under mild conditions and preparing regenerated cellulose fiber or film according to claim 1, characterized in that: The ionic liquid is selected from any one or a combination of at least two of 1-R2-3-R1-imidazole phosphite methyl (or ethyl, or butyl) ester and 1-R2-1,5-diazabicyclo[4.3.0]-5-nonene phosphite methyl (or ethyl, or butyl) ester, wherein R1, R2 = C m H 2n+1 , m and n are values ​​ranging from 1 to 10, and are both positive integers.

3. The method for dissolving cellulose with ionic liquid under mild conditions and preparing regenerated cellulose fiber or film according to claim 1, characterized in that: The cellulose may be one or more of microcrystalline cellulose, wood pulp cellulose, cotton pulp cellulose, mushroom grass cellulose, bamboo pulp cellulose, and paper pulp cellulose, and the degree of polymerization is between 220 and 2000.

4. The method for dissolving cellulose with ionic liquid under mild conditions and preparing regenerated cellulose fiber or film according to claim 1, wherein the ionic liquid aqueous solution used for swelling the cellulose is 40-80 wt%.

5. The method for dissolving cellulose with ionic liquid under mild conditions and preparing regenerated cellulose fiber or film according to claim 1, characterized in that: The mass ratio of the cellulose to the phosphite ionic liquid is (0.01-0.20):1, wherein the dissolution temperature is 50-80°C, the dissolution time is 3-8h, and the mechanical stirring speed is 100-300rpm.

6. The method for dissolving cellulose with ionic liquid under mild conditions and preparing regenerated cellulose fiber or film according to claim 1, characterized in that: The coagulation bath may be one or more of water, methanol, and ethanol.

7. The method for dissolving cellulose with ionic liquid under mild conditions and preparing regenerated cellulose fiber or film according to claims 1-6, characterized in that: The prepared regenerated cellulose fiber has a breaking strength of 1.2-2.5 cN / dtex and an elongation of 8%-13%, and the regenerated cellulose film has a tensile strength of 122.8-145.3 MPa and an elongation of 7.8-12.1%.

Citation Information

Patent Citations

  • Method for continuously preparing regenerated cellulose fibre

    CN101328626A

  • Anti-degradable solvent for dissolving cellulose and preparation method of spinning dope thereof

    CN101654522A

  • Preparation method of cellulose diacetate fiber

    CN102251302A

  • Method of using ionic liquid solvent system to dissolve fermented mushroom dregs to prepare polymers

    CN107573401A

  • Ionic liquid method regenerated cellulosic fiber and manufacturing method thereof

    CN109898169A

Cited By

  • Method for preparing composite film from biomass cellulose and composite film

    CN119350682A

  • Cellulose solution containing stabilizer as well as preparation method and application of cellulose solution

    CN121378802A