Preparation method of carbon fiber / phenolic resin composite material
By constructing a brick slurry structure on the surface of carbon fiber, the interface performance, ablation and thermal insulation of carbon fiber/phenolic resin composite materials are improved, and the problem of insufficient interface performance of existing materials in high-temperature environments is solved, thereby achieving higher thermal Protective performance and longer service life.
Patent Information
- Application Number
- CN202411010109.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The lack of interfacial performance of carbon fiber/phenolic resin composites in high-temperature hot flow environments limits their application under harsh conditions, especially poor ablation and thermal insulation, which affects the safety and service life of the aircraft.
Using a brick slurry structure with synergistic enhancement effect on the surface of carbon fiber, the chemical reaction of tannin acid, octa-amino cage polysilsesquioxane and concave-concave rock stones generates adherent polymers and metal oxides to improve interface performance , ablation properties and thermal insulation, simplify the process and reduce costs.
It significantly improves the interface performance, ablation performance and thermal insulation of carbon fiber/phenolic resin composite materials, extends the service life of thermal protection materials, enhances the safety and load-bearing capacity of the aircraft, and is suitable for aerospace and military thermal protection fields.
Smart Images

Figure CN118930928A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a method for preparing a carbon fiber / phenolic resin composite material. Background Art
[0002] Carbon fabric reinforced phenolic composites (CF / PR) have the advantages of light weight, high tensile strength, high carbon yield, and good mechanical properties, and are widely used in aerospace thermal protection systems. With the increase in the speed and flight distance of spacecraft, chemical erosion and thermal erosion caused by aerodynamic heating are becoming more and more serious. At the same time, aircraft face higher temperature environments in hypersonic operation environments, and high thermal conductivity thermal protection materials will seriously affect the safety and service life of aircraft. The limited ablative properties, poor interface properties, and high thermal conductivity of carbon fiber (CF) / phenolic resin (PR) ablative thermal protection composites limit their further application under harsh conditions of use. Therefore, it has become a top priority to improve the performance of CF / PR composites to meet the higher thermal protection needs of aircraft.
[0003] When composite materials are in a high-temperature heat flow environment, the interface of the composite material is the weakest area, which directly affects the stability of the composite material and the safety of the aircraft. At present, most studies focus on carbon fiber surface treatment to improve the interface performance, including fiber modification such as chemical grafting, physical coating treatment, and chemical vapor deposition. However, these modifications often only focus on the interface performance of carbon fiber composites, without considering the ablation and thermal insulation of carbon fiber composites. In recent years, the ablation and thermal insulation of carbon fiber composites have attracted widespread attention by preparing a coating that can form an anti-oxidation ceramic layer on carbon fiber fabrics, but the application of inorganic coatings will cause the interface performance of composite materials to deteriorate, thereby reducing the mechanical properties of composite materials. Carbon fiber composite materials used for load-bearing, ablation and thermal insulation should have good interface performance and thermal insulation in addition to good ablation. Good mechanical properties can effectively resist mechanical erosion in harsh environments on the one hand, and on the other hand, composite materials have a certain load-bearing capacity. Good thermal insulation can effectively block heat transfer inward, extend the service life of thermal protection materials, and protect the flight safety of aircraft. Therefore, the research and development of carbon fiber / phenolic resin composite materials that have excellent interface properties, ablative properties and thermal insulation properties to meet the needs of composite materials integrated with load-bearing and thermal protection in the aerospace or military fields has become a research hotspot in the field of ablative carbon fiber / phenolic resin composite materials. Summary of the invention
[0004] In order to solve the above technical problems, an embodiment of the present invention provides a method for preparing a carbon fiber / phenolic resin composite material.
[0005] To achieve the above object, the embodiments of the present invention adopt the following technical solutions:
[0006] The present invention provides a method for preparing a carbon fiber / phenolic resin composite material, comprising the following steps:
[0007] A. Desizing the carbon fiber by placing it in an organic solvent;
[0008] B. Immersing the carbon fiber desized in step A into a soaking solution containing tannic acid, octaamino cage-like polysilsesquioxane and attapulgite, and drying to obtain a modified carbon fiber;
[0009] C. Dissolving phenolic resin in an organic solvent to prepare an impregnation solution, and coating the impregnation solution on the modified carbon fiber in step B, and obtaining a prepreg after drying. The prepregs are stacked in sequence, and hot-pressed and cured to obtain a modified carbon fiber / phenolic resin composite material.
[0010] In some embodiments, in step A, the desizing treatment is specifically to heat the carbon fiber in acetone to remove the sizing agent on the surface of the carbon fiber, and then wash away excess acetone with deionized water and vacuum dry it.
[0011] In some embodiments, in step A, the mass ratio of the carbon fiber to the phenolic resin in step C is 1:1.
[0012] In some embodiments, in step B, the concentration of tannic acid is 0.5-4.0 g / L, the concentration of octaamino caged polysilsesquioxane is 0.5-4.0 g / L, and the concentration of attapulgite is 0.5 g / L.
[0013] In some embodiments, in step C, the phenolic resin includes at least one of a magnesium phenolic resin, a barium phenolic resin, and a boron phenolic resin.
[0014] In some embodiments, in step C, the organic solvent comprises at least one of ethanol, propanol and acetone.
[0015] In some embodiments, in step C, the mass ratio of the organic solvent to the phenolic resin is 1:2-4:1.
[0016] In some embodiments, in step C, the hot pressing curing process is divided into three stages: the temperature of the first stage is 100-120°C, the heating rate is 2°C / min, and the insulation time is 30-60min; the temperature of the second stage is 140-160°C, the heating rate is 2°C / min, and the insulation time is 60-120min; the temperature of the third stage is 180-220°C, the heating rate is 2°C / min, and the insulation time is 60-180min.
[0017] The present invention achieves the improvement of the interface performance, ablation performance and thermal insulation of the carbon fiber / phenolic resin composite material by constructing a brick-paste structure with synergistic reinforcement on the surface of carbon fiber, and simplifies the process and reduces the cost. Tannic acid and octaamino caged polysilsesquioxane can undergo Michael addition and Schiff base reaction to generate a polymer with adhesion, and tannic acid can react chemically with attapulgite. Therefore, tannic acid, octaamino caged polysilsesquioxane and attapulgite can generate a brick-paste structure with tannic acid and octaamino caged polysilsesquioxane as "paste" and attapulgite as "brick" on the surface of carbon fiber under an alkaline environment. The construction of the brick-paste structure improves the fiber interface roughness and surface energy, and enhances the mechanical interlocking of the carbon fiber and the phenolic resin matrix through a multi-scale interface, which significantly improves the interface performance of the carbon fiber / phenolic resin composite material. At the same time, the multi-scale porous structure of the brick-paste structure gives the carbon fiber / phenolic resin composite material good thermal insulation. In addition, octaamino cage-like polysilsesquioxane and attapulgite can generate metal oxides and ceramics at high temperatures, which effectively improve the high-temperature oxidation resistance and ablation resistance of carbon fiber / phenolic resin composites.
[0018] In addition, the preparation process of the present invention is simple, the preparation time is short, the production cost is low, and mass production is easy to achieve; the modification of carbon fiber by the present invention does not involve strong oxidants and strong acids, is green and environmentally friendly, and does not damage the carbon fiber; the brick slurry structure constructed by the present invention further improves the interface roughness and high temperature resistance, and the composite material prepared by the present invention also has good interface properties, ablation properties and thermal insulation properties, and has broad application prospects in the fields of aerospace and military thermal protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The SEM images of carbon fibers modified by Examples 1 to 5 and Comparative Examples 2 and 3, wherein (a) is a SEM image of carbon fibers modified by Example 5, (b) is a SEM image of carbon fibers modified by Example 1, (c) is a SEM image of carbon fibers modified by Example 2, (d) is a SEM image of carbon fibers modified by Example 3, (e) is a SEM image of carbon fibers modified by Example 4, (f) is a SEM image of carbon fibers modified by Comparative Example 2, and (g) is a SEM image of carbon fibers modified by Comparative Example 3;
[0020] Figure 2 The SEM images of the interface failure of the samples of Comparative Example 2, Comparative Example 3 and Example 6, wherein (a) is the SEM image of the interface failure of the sample of Comparative Example 2, (b) is the SEM image of the interface failure of the sample of Comparative Example 3, and (c) is the SEM image of the interface failure of the sample of Example 6;
[0021] Figure 3Surface morphology of the modified carbon fiber / phenolic resin composite material sample after ablation, wherein (a) and (d) are surface morphology of the modified carbon fiber / phenolic resin composite material sample after ablation of Comparative Example 2, (b) and (e) are surface morphology of the modified carbon fiber / phenolic resin composite material sample after ablation of Comparative Example 3, (c) and (f) are surface morphology of the modified carbon fiber / phenolic resin composite material sample after ablation of Example 6;
[0022] Figure 4 This is a SEM image of the modified carbon fiber / phenolic resin composite material sample after ablation prepared in Comparative Example 2;
[0023] Figure 5 This is a SEM image of the modified carbon fiber / phenolic resin composite material sample after ablation prepared in Comparative Example 3;
[0024] Figure 6 This is a SEM image of the modified carbon fiber / phenolic resin composite material sample after ablation obtained in Example 6;
[0025] Figure 7 This is the EDS image of the modified carbon fiber / phenolic resin composite material sample after ablation prepared in Comparative Example 2;
[0026] Figure 8 This is the EDS image of the modified carbon fiber / phenolic resin composite material sample after ablation prepared in Comparative Example 3;
[0027] Fig. 9 This is the EDS image of the modified carbon fiber / phenolic resin composite material sample prepared in Example 6 after ablation. DETAILED DESCRIPTION
[0028] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in some embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all the embodiments. Based on the embodiments provided by the present disclosure, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present disclosure.
[0029] Example 1
[0030] The carbon fiber was soaked in acetone for 72 hours, and after the excess acetone was washed off with deionized water, it was placed in a vacuum oven and dried at 80°C for 10 hours to obtain desizing carbon fiber; the desizing carbon fiber was immersed in a mixture containing 0.5g / L tannic acid, 2g / L octaamino caged polysilsesquioxane and 0.5g / L attapulgite, and soaked for 4 hours, and dried at 80°C to obtain modified carbon fiber, and the boron phenolic resin was poured into anhydrous ethanol of equal mass, and mechanically stirred and mixed at room temperature to obtain an impregnation solution. The impregnation solution was evenly applied to the carbon fiber fabric by hand paste method (the mass ratio of carbon fiber to boron phenolic resin was 1:1), and then dried at room temperature to form a prepreg; the obtained carbon fiber prepreg was stacked and placed in a vulcanizer. The temperature was kept at 120℃ for 1h under 5MPa pressure, the heating rate was 2℃ / min, the temperature was raised to 150℃ for 1h, the temperature was raised to 180℃ for 2h, the temperature was raised to 200℃ for 1h at a heating rate of 2℃ / min, and the temperature was finally raised to 200℃ for 1h. The press was finally cooled and demoulded to obtain a modified carbon fiber / phenolic resin composite material.
[0031] Example 2
[0032] The carbon fiber was soaked in acetone for 72 hours, and after the excess acetone was washed off with deionized water, it was placed in a vacuum oven and dried at 80°C for 10 hours to obtain desizing carbon fiber; the desizing carbon fiber was immersed in a mixture containing 1g / L tannic acid, 2g / L octaamino caged polysilsesquioxane and 0.5g / L attapulgite, and soaked for 4 hours, and dried at 80°C to obtain modified carbon fiber, and the boron phenolic resin was poured into anhydrous ethanol of equal mass, and mechanically stirred and mixed at room temperature to obtain an impregnation solution. The impregnation solution was evenly applied to the carbon fiber fabric by hand paste method (the mass ratio of carbon fiber to boron phenolic resin was 1:1), and then dried at room temperature to form a prepreg; the obtained carbon fiber prepreg was stacked and placed in a vulcanizer. The temperature was kept at 120℃ for 1h under 5MPa pressure, the heating rate was 2℃ / min, the temperature was raised to 150℃ for 1h, the temperature was raised to 180℃ for 2h, the temperature was raised to 200℃ for 1h at a heating rate of 2℃ / min, and the temperature was finally raised to 200℃ for 1h. The press was finally cooled and demoulded to obtain a modified carbon fiber / phenolic resin composite material.
[0033] Example 3
[0034] The carbon fiber was soaked in acetone for 72 hours, and after the excess acetone was washed off with deionized water, it was placed in a vacuum oven and dried at 80°C for 10 hours to obtain desizing carbon fiber; the desizing carbon fiber was immersed in a mixture containing 2g / L tannic acid, 1g / L octaamino caged polysilsesquioxane and 0.5g / L attapulgite for 4 hours, and dried at 80°C to obtain the modified carbon fiber, and the boron phenolic resin was poured into anhydrous ethanol of equal mass, and mechanically stirred and mixed at room temperature to obtain the impregnation solution. The impregnation solution was evenly applied to the carbon fiber fabric by hand paste method (the mass ratio of carbon fiber to boron phenolic resin was 1:1), and then dried at room temperature to form a prepreg; the obtained carbon fiber prepreg was stacked and placed in a vulcanizer. The temperature was kept at 120℃ for 1h under 5MPa pressure, the heating rate was 2℃ / min, the temperature was raised to 150℃ for 1h, the temperature was raised to 180℃ for 2h, the temperature was raised to 200℃ for 1h at a heating rate of 2℃ / min, and the temperature was finally raised to 200℃ for 1h. The press was finally cooled and demoulded to obtain a modified carbon fiber / phenolic resin composite material.
[0035] Example 4
[0036] The carbon fiber was soaked in acetone for 72 hours, and after the excess acetone was washed off with deionized water, it was placed in a vacuum oven and dried at 80°C for 10 hours to obtain desizing carbon fiber; the desizing carbon fiber was immersed in a mixture containing 2g / L tannic acid, 0.5g / L octaamino caged polysilsesquioxane and 0.5g / L attapulgite, and soaked for 4 hours, and dried at 80°C to obtain modified carbon fiber, and the boron phenolic resin was poured into anhydrous ethanol of equal mass, and mechanically stirred and mixed at room temperature to obtain an impregnation solution. The impregnation solution was evenly applied to the carbon fiber fabric by hand paste method (the mass ratio of carbon fiber to boron phenolic resin was 1:1), and then dried at room temperature to form a prepreg; the obtained carbon fiber prepreg was stacked and placed in a vulcanizer. The temperature was kept at 120℃ for 1h under 5MPa pressure, the heating rate was 2℃ / min, the temperature was raised to 150℃ for 1h, the temperature was raised to 180℃ for 2h, the temperature was raised to 200℃ for 1h at a heating rate of 2℃ / min, and the temperature was finally raised to 200℃ for 1h. The press was finally cooled and demoulded to obtain a modified carbon fiber / phenolic resin composite material.
[0037] Example 5
[0038] The carbon fiber was soaked in acetone for 72 hours, and after the excess acetone was washed off with deionized water, it was placed in a vacuum oven and dried at 80°C for 10 hours to obtain desized carbon fiber; the desized carbon fiber was immersed in a mixed solution containing 2g / L tannic acid, 2g / L octaamino caged polysilsesquioxane and 0.5g / L attapulgite, soaked for 4 hours, and dried at 80°C to obtain modified carbon fiber; the boron phenolic resin was poured into anhydrous ethanol of equal mass, and mechanically stirred and mixed at room temperature to obtain an impregnation solution. The impregnation solution was evenly applied to the carbon fiber fabric by hand-paste method (the mass ratio of carbon fiber to boron phenolic resin was 1:1), and then dried at room temperature to form a prepreg; the obtained carbon fiber prepreg was stacked and placed in a vulcanizer. Under 5MPa pressure, keep the temperature at 120℃ for 1h, the heating rate is 2℃ / min, then heat to 150℃ for 1h, the heating rate is 2℃ / min, heat to 180℃ for 2h, and finally heat to 200℃ for 1h at a heating rate of 2℃ / min. Finally, the press is cooled and demoulded to obtain a modified carbon fiber / phenolic resin composite material. The interlaminar shear strength of the obtained sample at room temperature is 37.41MPa; the interlaminar shear strength after high temperature oxidation is 2.41MPa; the linear ablation rate of oxygen-acetylene is -0.0068mm / s, the mass ablation rate is 0.035g / s; the thermal conductivity is 1.14W / m·K.
[0039] Example 6
[0040] The carbon fiber was soaked in acetone for 72 hours, and after the excess acetone was washed off with deionized water, it was placed in a vacuum oven and dried at 80°C for 10 hours to obtain desized carbon fiber; the desized carbon fiber was immersed in a mixture containing 2g / L tannic acid, 2g / L octaamino caged polysilsesquioxane and 0.5g / L attapulgite, soaked for 8 hours, and dried at 80°C to obtain modified carbon fiber; the boron phenolic resin was dissolved in anhydrous ethanol of equal mass, and mechanically stirred and mixed at room temperature to obtain an impregnation solution. The impregnation solution was evenly applied to the carbon fiber fabric by hand paste method, and the fiber was thoroughly impregnated with a brush, and then dried at room temperature to form a prepreg; the obtained carbon fiber prepreg was stacked and placed in a vulcanizer. Under 5MPa pressure, keep the temperature at 120℃ for 1h, the heating rate is 2℃ / min, then heat to 150℃ for 1h, the heating rate is 2℃ / min, heat to 180℃ for 2h, and finally heat to 200℃ for 1h at a heating rate of 2℃ / min. Finally, the press is cooled and demoulded to obtain a modified carbon fiber / phenolic resin composite material. The interlaminar shear strength of the obtained sample at room temperature is 38.43MPa; the interlaminar shear strength after high-temperature oxidation is 2.65MPa; the oxygen-acetylene linear ablation rate is -0.013mm / s, the mass ablation rate is 0.032g / s; the thermal conductivity is 1.04W / m·K.
[0041] Example 7
[0042] The carbon fiber was soaked in acetone for 72 hours, and after the excess acetone was washed off with deionized water, it was placed in a vacuum oven and dried at 80°C for 10 hours to obtain desized carbon fiber; the desized carbon fiber was immersed in a mixture containing 2g / L tannic acid, 2g / L octaamino caged polysilsesquioxane and 0.5g / L attapulgite, and soaked for 12 hours, and dried at 80°C to obtain modified carbon fiber; the boron phenolic resin was poured into anhydrous ethanol of equal mass, and mechanically stirred and mixed at room temperature to obtain an impregnation solution. The impregnation solution was evenly applied to the carbon fiber fabric by hand paste method, and the fiber was thoroughly impregnated with a brush, and then dried at room temperature to form a prepreg; the obtained carbon fiber prepreg was stacked and placed in a vulcanizer. Under 5MPa pressure, keep the temperature at 120℃ for 1h, the heating rate is 2℃ / min, then heat to 150℃ for 1h, the heating rate is 2℃ / min, heat to 180℃ for 2h, and finally heat to 200℃ for 1h at a heating rate of 2℃ / min. Finally, the press is cooled and demoulded to obtain a modified carbon fiber / phenolic resin composite material. The interlaminar shear strength of the obtained sample at room temperature is 37.11MPa; the interlaminar shear strength after high temperature oxidation is 2.92MPa; the oxygen-acetylene linear ablation rate is 0.0075mm / s, the mass ablation rate is 0.032g / s; the thermal conductivity is 1.08W / m·K.
[0043] Comparative Example 1: Preparation of carbon fiber / phenolic resin composite material
[0044] The boron phenolic resin was dissolved in anhydrous ethanol of equal mass, and the mixture was mechanically stirred and mixed at room temperature to obtain an impregnation solution. The impregnation solution was evenly applied to the carbon fiber by hand paste method, and then dried at room temperature to form a prepreg; the obtained carbon fiber prepreg was stacked and placed in a vulcanizer. Under a pressure of 5MPa, the temperature was kept at 120℃ for 1h, the heating rate was 2℃ / min, the temperature was increased to 150℃ for 1h, the heating rate was 2℃ / min, the temperature was increased to 180℃ for 2h, and finally the heating rate was 2℃ / min, the temperature was increased to 200℃ for 1h. Finally, the press was cooled and demolded to obtain a modified carbon fiber / phenolic resin composite material. The interlaminar shear strength of the obtained sample at room temperature was 31.01MPa; the interlaminar shear strength after high temperature oxidation was 1.58MPa; the linear ablation rate of oxygen-acetylene was 0.042mm / s, the mass ablation rate was 0.038g / s; the thermal conductivity was 1.11W / m·K.
[0045] Comparative Example 2: Preparation of desized carbon fiber / phenolic resin composite material
[0046] The carbon fiber was soaked in acetone for 72 hours, and after the excess acetone was washed off with deionized water, it was placed in a vacuum oven and dried at 80°C for 10 hours to obtain the modified carbon fiber; the boron phenolic resin was poured into anhydrous ethanol of equal mass, and mechanically stirred and mixed at room temperature to obtain an impregnation solution. The impregnation solution was evenly applied to the modified carbon fiber by hand paste method, and then dried at room temperature to form a prepreg; the obtained carbon fiber prepreg was stacked and placed in a vulcanizer. Under a pressure of 5MPa, it was kept at 120°C for 1 hour, the heating rate was 2°C / min, the temperature was raised to 150°C for 1 hour, the heating rate was 2°C / min, the temperature was raised to 180°C for 2 hours, and finally the heating rate was 2°C / min, and the temperature was raised to 200°C for 1 hour. Finally, the press was cooled and demolded to obtain a modified carbon fiber / phenolic resin composite material. The interlaminar shear strength of the obtained sample at room temperature is 28.09MPa; the interlaminar shear strength after high-temperature oxidation is 2.48MPa; the oxygen-acetylene linear ablation rate is 0.0083mm / s, the mass ablation rate is 0.038g / s; and the thermal conductivity is 1.21W / m·K.
[0047] Comparative Example 3: Preparation of co-deposition modified carbon fiber / phenolic resin composite material
[0048] Soak the carbon fiber in acetone for 72 hours, wash off the excess acetone with deionized water, and dry it in a vacuum oven at 80°C for 10 hours to obtain a desized carbon fiber cloth; immerse the desized carbon fiber in a mixed solution containing 2g / L tannic acid and 2g / L octaamino caged polysilsesquioxane for 12 hours, and dry it at 80°C to obtain a co-deposited modified carbon fiber; pour the boron phenolic resin and into anhydrous ethanol of equal mass, and mix them evenly by mechanical stirring at room temperature to obtain an impregnation solution. Use the hand paste method to evenly apply the impregnation solution on the modified carbon fiber, thoroughly impregnate the fiber with a brush, and then dry it at room temperature to form a prepreg; stack the obtained carbon fiber prepreg and put it into a vulcanizer. Under 5MPa pressure, keep the temperature at 120℃ for 1h, the heating rate is 2℃ / min, then heat to 150℃ for 1h, the heating rate is 2℃ / min, heat to 180℃ for 2h, and finally heat to 200℃ for 1h at a heating rate of 2℃ / min. Finally, cool and demould with the press to obtain the co-deposited modified carbon fiber / phenolic resin composite material. The interlaminar shear strength of the obtained sample at room temperature is 36.51MPa; the bending strength and interlaminar shear strength after high temperature oxidation are 2.46MPa; the linear ablation rate of oxygen-acetylene is 0.0078mm / s, the mass ablation rate is 0.038g / s; the thermal conductivity is 1.08W / m·K.
[0049] Through the comparison of the embodiments and comparative examples, it is concluded that compared with carbon fiber / phenolic resin and co-deposition modified carbon fiber composites, the construction of the brick mortar structure significantly improves the ablation, interface and thermal insulation of the composite material. The modification of the brick mortar structure improves the fiber interface roughness and surface energy, and enhances the mechanical interlocking of the carbon fiber and the phenolic resin matrix through the multi-scale interface, thereby improving the mechanical properties of the composite material. At the same time, the multi-scale porous structure of the brick mortar structure gives the carbon fiber composite material good thermal insulation. In addition, octaamino cage-like polysilsesquioxane and attapulgite can generate metal oxides and ceramics at high temperatures, effectively improving the high-temperature oxidation resistance and ablation resistance of carbon fiber.
[0050] Although the co-deposition structure can effectively improve the interface performance of the composite material, the presence of a large amount of organic matter promotes the thermal decomposition of the phenolic resin matrix during the ablation process, resulting in poor ablation performance of the composite material. The brick mortar structure introduces inorganic materials to improve the high temperature resistance of the interface, while the construction of a multi-scale porous structure further enhances the thermal insulation of the composite material. Figure 1 It was confirmed that the brick-paste structure was successfully constructed on the carbon fiber surface; Figure 2 It shows that the construction of brick-paste structure can effectively improve the interfacial bonding strength of carbon fiber composites; Figure 3 It shows that the microscopic morphology of the carbon fiber after ablation of the composite material prepared in Example 6 is more complete and there are adhesive substances, which further shows that the construction of the brick mortar structure can effectively improve the high temperature oxidation resistance of the carbon fiber, thereby improving the ablation property of the composite material;, Figure 4-Figure 6 The central morphologies of the samples of Comparative Example 2, Comparative Example 3 and Example 6 after ablation are shown in the figure. It can be observed from the figure that the fiber morphology after ablation is greatly damaged, and the presence of ceramic protective phase can be observed on the carbon fibers after co-deposition modification and brick slurry structure modification. Figure 7-Figure 9 The corresponding EDS spectrum further confirms the existence of the ceramic protective phase. Combined with the ablation performance of Comparative Example 2, Comparative Example 3 and Example 6, it is further proved that the generation of inorganic substances on the carbon fiber surface effectively improves the ablation of the carbon fiber. In addition, due to the better interface performance of the brick mortar structure, there is more resin matrix in the composite material of Example 6, which better protects the carbon fiber from oxidation and improves the ablation performance of the composite material.
[0051] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.
[0052] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a carbon fiber / phenolic resin composite material, characterized in that: The following steps are involved: A. Desizing the carbon fiber by placing it in an organic solvent; B. Immersing the carbon fiber desized in step A into a soaking solution containing tannic acid, octaamino cage-like polysilsesquioxane and attapulgite, and drying to obtain a modified carbon fiber; C. Dissolving phenolic resin in an organic solvent to prepare an impregnation solution, and coating the impregnation solution on the modified carbon fiber in step B, and obtaining a prepreg after drying. The prepregs are stacked in sequence, and hot-pressed and cured to obtain a modified carbon fiber / phenolic resin composite material.
2. The preparation method according to claim 1, characterized in that: In step A, the desizing treatment is specifically to heat the carbon fibers in acetone to remove the sizing agent on the surface of the carbon fibers, and then to wash away excess acetone with deionized water and then to dry in vacuum.
3. The preparation method according to claim 1, characterized in that: In step A, the mass ratio of the carbon fiber to the phenolic resin in step C is 1:
1.
4. The preparation method according to claim 1, characterized in that: In step B, the concentration of tannic acid is 0.5-4.0 g / L, the concentration of octaamino caged polysilsesquioxane is 0.5-4.0 g / L, and the concentration of attapulgite is 0.5 g / L.
5. The preparation method according to claim 1, characterized in that: In step C, the phenolic resin includes at least one of a magnesium phenolic resin, a barium phenolic resin and a boron phenolic resin.
6. The preparation method according to claim 1, characterized in that: In step C, the organic solvent includes at least one of ethanol, propanol and acetone.
7. The preparation method according to claim 1, characterized in that: In step C, the mass ratio of the organic solvent to the phenolic resin is 1:2-4:
1.
8. The preparation method according to claim 1, characterized in that: In step C, the hot pressing curing process is divided into three stages: the temperature of the first stage is 100-120°C, the heating rate is 2°C / min, and the insulation time is 30-60min; the temperature of the second stage is 140-160°C, the heating rate is 2°C / min, and the insulation time is 60-120min; the temperature of the third stage is 180-220°C, the heating rate is 2°C / min, and the insulation time is 60-180min.
Citation Information
Patent Citations
Carbon / phenolic heat insulating composite material and manufacturing process thereof
CN101440193A
Modified carbon fiber reinforced phenolic resin-based composite material and preparation thereof
CN110938281A
Modified carbon fiber / phenolic resin composite material and preparation method thereof
CN114874470A
Antioxidant ablation-resistant coating and preparation method thereof
CN115851070A
Modified carbon fiber, preparation method thereof and application of modified carbon fiber in enhancing mechanical properties of composite material
CN116590921A
Cited By
Ablation-resistant aramid fiber / phenolic resin composite material and preparation method thereof
CN122344382A
Aramid fiber / phenolic resin composite material resistant to ablation and a preparation method thereof
CN122344382B