Microporous fluoroelastomer composition and preparation method thereof

Through pre-sulfurization molding, physical foaming molding, radiation vulcanization crosslinking and secondary vulcanization crosslinking, the problems of micropore merger and low production efficiency caused by traditional high-temperature vulcanization crosslinking are solved, and high-strength, ozone-resistant micro-micro-micro-weighted, resistant to ozone are prepared The porous fluoroelastomer composition achieves a smaller cell size and a more uniform structure and efficient production.

CN118930945APending Publication Date: 2024-11-12SHANGHAI MORISEAL NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411087658.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional high-temperature vulcanization cross-linking methods cause the micropores of the microporous fluoroelastomer composition to become larger during the long-term vulcanization process, which affects performance, has low production efficiency and large energy consumption.

Method used

Using pre-sulfurization molding - physical foaming shaping - radiation vulcanization crosslinking - secondary vulcanization crosslinking, supercritical carbon dioxide foaming and radiation vulcanization crosslinking, the smaller cell size and better through high pressure or supercritical fluids. A uniform cell structure, and radiation vulcanization cross-linking and secondary high-temperature vulcanization are performed at room temperature to shorten the vulcanization time.

Benefits of technology

A high-strength, ozone-resistant microporous fluoroelastomer composition was prepared, which stabilized the microporous structure, improved performance, shortened production time and reduced energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930945A_ABST
    Figure CN118930945A_ABST
Patent Text Reader

Abstract

The invention provides a microporous fluoroelastomer composition and a preparation method thereof, and belongs to the field of fluoroelastomers, and the preparation method specifically comprises the following steps: step 1, pre-vulcanization molding; step 2, physical shaping; step 3, foaming and shaping: putting the non-microporous and non-secondary-vulcanized fluoroelastomer composition into a forming mold, and carrying out rapid pressure reduction and expansion after the non-microporous and non-secondary-vulcanized fluoroelastomer composition and the forming mold reach dissolution equilibrium in the forming mold by adopting high-pressure or supercritical fluid, cooling and shaping to obtain a microporous fluoroelastomer composition which is not secondarily vulcanized; 4, radiation vulcanization crosslinking: carrying out radiation vulcanization crosslinking on the microporous and unvulcanized fluoroelastomer composition to obtain a crosslinked fluoroelastomer composition; and step 5, secondary vulcanization crosslinking: performing secondary vulcanization on the crosslinked fluoroelastomer composition to obtain the microporous fluoroelastomer composition. According to the treatment scheme, the prepared microporous fluoroelastomer composition has the advantages of high strength, ozone resistance and uniform foaming.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fluoroelastomers, and in particular to a microporous fluoroelastomer composition and a preparation method thereof. Background Art

[0002] Fluoroelastomer compositions are widely used in sealing, insulating and protective materials in the fields of chemical industry, nuclear industry, etc. The properties of fluoroelastomer compositions depend on the selected formula and processing technology. The vulcanization process is a very critical link in the processing technology, including high-temperature vulcanization cross-linking and room-temperature radiation vulcanization cross-linking. High-temperature vulcanization cross-linking is a commonly used method that uses a vulcanizing agent for cross-linking at high temperature. It requires a long vulcanization time, and the microbubbles are easy to break and grow, affecting the performance of the elastomer. In addition, the energy consumption is relatively large.

[0003] Porous structure fluororubber refers to a material with a fluoroelastomer as the matrix and a large number of bubbles or pores inside. It can also be regarded as a fluoroelastomer composite material with gas as the filler. Compared with bulk fluororubber, porous structure fluororubber can reduce the amount of material while not affecting or even expanding the material performance, thereby achieving the purpose of reducing costs and improving cost performance.

[0004] When preparing porous fluoroelastomer compositions, the existing traditional high-temperature crosslinking has the following problems: The traditional high-temperature vulcanization cross-linking method requires a long vulcanization time, which reduces production efficiency and consumes a lot of energy. At the same time, the traditional high-temperature vulcanization cross-linking method easily causes the micropores in the microporous elastomer composition to merge and become larger during the long vulcanization process, affecting the performance of the microporous elastomer composition.

[0005] Therefore, it is necessary to provide a new preparation method to solve these problems. Summary of the invention

[0006] Therefore, in order to overcome the above-mentioned disadvantages of the prior art, the present invention provides a microporous fluoroelastomer composition with high strength, ozone resistance and uniform foaming and a preparation method thereof.

[0007] In order to achieve the above-mentioned object, the present invention provides a method for preparing a microporous fluoroelastomer composition, comprising: step 1 pre-vulcanization molding: mixing 100 parts by weight of fluoroelastomer with 5 to 25 parts of nucleating agent, 0 to 20 parts of filler, and 0 to 10 parts of acid absorbent to obtain a fluoroelastomer rubber mix; step 2 physical shaping: molding the fluoroelastomer rubber mix to obtain a non-microporous and non-secondary vulcanized fluoroelastomer composition; step 3 foaming shaping: placing the non-microporous and non-secondary vulcanized fluoroelastomer composition In the molding die, a high pressure or supercritical fluid is used to make the non-microporous and non-secondary-vulcanized fluoroelastomer composition reach a dissolution equilibrium with the fluid in the molding die, and then the pressure is rapidly reduced and expanded, and the microporous but non-secondary-vulcanized fluoroelastomer composition is obtained by cooling and setting; step 4: radiation vulcanization and crosslinking: the microporous but non-secondary-vulcanized fluoroelastomer composition is subjected to radiation vulcanization and crosslinking to obtain a crosslinked fluoroelastomer composition; step 5: secondary vulcanization and crosslinking: the crosslinked fluoroelastomer composition is subjected to secondary vulcanization to obtain a microporous fluoroelastomer composition.

[0008] In one embodiment, the radiation vulcanization cross-linking in step 4 is performed at room temperature using a linear electron accelerator, and the radiation dose is 15-100 kGy.

[0009] In one embodiment, the fluoroelastomer is a copolymer formed by vinylidene fluoride, a vulcanization site monomer and at least one of the following monomers: tetrafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, and perfluorophenoxypropyl vinyl ether.

[0010] In one embodiment, the nucleating agent includes at least one of talc, calcium carbonate, calcium stearate, zinc stearate, sodium benzoate, magnesium oxide, silicon dioxide, boron nitride, and PTFE particles (polytetrafluoroethylene particles).

[0011] In one embodiment, the filler includes at least one of carbon nanotubes, carbon black, graphene, silicon dioxide and titanium dioxide.

[0012] In one embodiment, the acid absorber includes at least one of MaO, Ca(OH)2, ZnO, and CaO.

[0013] In one embodiment, 1-2 parts of a vulcanizing agent and 0.3-3 parts of an accelerator are further added in step 1, wherein the vulcanizing agent includes at least one of bisphenol AF, di-tert-butyl peroxide isopropylbenzene, and dipentadienyl vulcanizing agent, and the accelerator is at least one of benzyltriphenylphosphine chloride (BPP accelerator) and triallyl isocyanurate (TAIC).

[0014] In one embodiment, in step 2, the compression molding conditions are 8-10 MPa, 160-175° C., and 5-16 min.

[0015] In one embodiment, in step 3, the rapid pressure relief and expansion time is 1 to 15 s, preferably 2 to 10 s.

[0016] In one embodiment, in step 3, the component of the high pressure or supercritical fluid is carbon dioxide or nitrogen, the pressure in the autoclave is 8-40 MPa, and the temperature is 60-140°C.

[0017] In one embodiment, the secondary vulcanization condition in step 5 is 200-220° C., 0.5-4 hr.

[0018] A microporous fluoroelastomer composition is prepared by the above method.

[0019] Compared with the prior art, the advantages of the present invention are: using the process of "pre-vulcanization molding - physical foaming shaping - radiation vulcanization cross-linking - secondary vulcanization cross-linking", using supercritical carbon dioxide foaming and radiation vulcanization cross-linking to prepare a high-strength, ozone-resistant microporous fluoroelastomer composition. High pressure or supercritical fluid is used as a physical foaming agent to obtain a smaller cell size and a more uniform cell structure; and room temperature radiation vulcanization cross-linking is used to stabilize the microporous structure and a short time of secondary vulcanization, shortening the vulcanization production time, reducing the amount of vulcanizer and vulcanization accelerator used, making the microporous structure stable, thereby ensuring that the fluoroelastomer composition has strong ozone resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 It is a flow chart of the preparation method of the microporous fluoroelastomer composition in the embodiment of the present invention. DETAILED DESCRIPTION

[0022] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0023] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0024] It should be noted that various aspects of the embodiments within the scope of protection of the present invention are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0025] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0026] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0027] like Figure 1 As shown, the present embodiment provides a method for preparing a microporous fluoroelastomer composition, comprising: S1 pre-vulcanization molding: 100 parts by weight of fluoroelastomer, 5-25 parts by weight of nucleating agent, 0-20 parts by weight of filler, and 0-10 parts by weight of acid absorbent are mixed and kneaded to obtain a fluoroelastomer compound rubber.

[0028] The selection criteria for fluoroelastomers may be elastomers containing PVDF. Since there is a lot of solubility research data on supercritical CO2-PVDF-containing fluoropolymer systems, the crystallinity of the composition changes only slightly during the swelling process, which is conducive to expansion and foaming.

[0029] Thin-pass mixing is to adjust the roller gap of the open mixing mill to 1.2-3.5 mm, allow the above-mentioned weight proportions of rubber components to pass through the roller gap, and allow them to fall into the receiving plate. After all the rubber has passed through the roller gap, the rubber on the plate is folded twice and then thin-passed. After a period of time, such as 40 minutes, vulcanizers and vulcanizing aids are added, and thin-pass mixing is continued until the surface of the mixed rubber is flat and free of particles. The total time for thin-pass mixing is about 1 hour.

[0030] In one embodiment, the fluoroelastomer is a copolymer formed by vinylidene fluoride, a cure site monomer and at least one of the following monomers: tetrafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, and perfluorophenoxypropyl vinyl ether.

[0031] In one embodiment, the nucleating agent includes at least one of talc, calcium carbonate, calcium stearate, zinc stearate, sodium benzoate, magnesium oxide, silicon dioxide, boron nitride, and PTFE particles.

[0032] In one embodiment, the filler includes at least one of carbon nanotubes, carbon black, graphene, silicon dioxide and titanium dioxide.

[0033] In one embodiment, the acid absorber includes at least one of MaO, Ca(OH)2, ZnO, and CaO.

[0034] S2 physical shaping: the fluoroelastomer compound is molded to obtain a fluoroelastomer composition that is not microporous and not secondary vulcanized.

[0035] The fluoroelastomer compound is molded to obtain a non-microporous and non-secondary vulcanized fluoroelastomer composition. The molding conditions are 7-12 MPa, 150-185°C, and 5-20 min. Preferably, in step 2, the molding conditions are 8-10 MPa, 160-175°C, and 5-16 min.

[0036] S3 Foaming and shaping: Place the non-microporous and non-secondary vulcanized fluoroelastomer composition in a molding mold, use high pressure or supercritical fluid to make the non-microporous and non-secondary vulcanized fluoroelastomer composition reach dissolution equilibrium with the mold, then rapidly reduce pressure and expand, cool and shape to obtain a microporous but non-secondary vulcanized fluoroelastomer composition.

[0037] A non-microporous and non-secondarily vulcanized fluoroelastomer composition is placed in a molding die, sealed in an autoclave, and the air is replaced and the pressure is increased by using a high-pressure or supercritical fluid, and the temperature and pressure in the autoclave are controlled. After the high-pressure or supercritical fluid reaches or approaches a dissolution equilibrium in the non-microporous and non-secondarily vulcanized fluoroelastomer composition, heating is stopped and the pressure is quickly released to allow the non-microporous and non-secondarily vulcanized fluoroelastomer composition to expand in the molding die, and the microporous but non-secondarily vulcanized fluoroelastomer composition is obtained by cooling and shaping.

[0038] A non-microporous and non-secondarily vulcanized fluoroelastomer composition is placed in a molding mold, sealed in an autoclave, and the air is replaced by a high-pressure or supercritical fluid and the pressure is increased. At this time, the high-pressure or supercritical fluid and the fluoroelastomer composition form a two-phase system.

[0039] The temperature and pressure in the autoclave are controlled, and the high-pressure or supercritical fluid swells the fluoroelastomer composition, and the high-pressure or supercritical fluid reaches or approaches a dissolution equilibrium in the fluoroelastomer composition that is not microporous and not post-cured.

[0040] Stop heating, open the valve and reduce the pressure sharply to make the non-microporous and non-secondary-cured fluoroelastomer composition expand in the molding die. Under the induction of the nucleating agent, the high pressure or supercritical fluid forms bubbles in the non-microporous and non-secondary-cured fluoroelastomer composition; the bubbles grow and merge. Cool and shape to obtain a microporous but non-secondary-cured fluoroelastomer composition.

[0041] In one embodiment, the high pressure or supercritical fluid is carbon dioxide or nitrogen. For example, the critical temperature of CO2 fluid is 31.26°C and the critical pressure is 72.9 atm; the critical temperature of N2 fluid is -147°C and the critical pressure is 33.5 atm.

[0042] S4 Radiation vulcanization crosslinking: Radiation vulcanization crosslinking the microvoided but not post-vulcanized fluoroelastomer composition to obtain a crosslinked fluoroelastomer composition.

[0043] There are about 3000 kinds of radiation that can directly or indirectly ionize the air, and any one of them can be selected. The radiation vulcanization crosslinking can be electron beam vulcanization crosslinking or gamma ray radiation vulcanization crosslinking.

[0044] Electron beam radiation vulcanization technology uses high-energy electron beams emitted by electron accelerators to activate elastomer molecules in the elastomer matrix, generate elastomer macromolecular free radicals, and cross-link elastomer macromolecules to form a three-dimensional network structure. In addition to ions, electrons, and excited molecules, the primary chemical products formed by radiation also include free radicals and certain molecular products. These primary particles are highly active and can undergo a variety of reactions such as cracking, rearrangement, electron transfer, dehydrogenation, and addition.

[0045] The radiation dose has a great influence on the performance of the elastomer composition, and the radiation effect is a competitive mechanism. When the rubber is irradiated, the intermolecular crosslinking reaction and the degradation reaction occur simultaneously, that is, on the one hand, the molecular weight of the network macromolecules formed by intermolecular crosslinking continues to increase; on the other hand, the radiation causes the chemical bonds to break and the relative molecular weight to decrease. Therefore, the radiation dose is an important parameter for determining the radiation vulcanization and crosslinking process of the elastomer composition. The radiation dose ranges from 15 to 100 kGy. Radiation is calculated by dose. When doing the experiment, the sample is placed on the turntable, and the dose is calculated once, and finally the total dose is calculated according to the number of times.

[0046] Radiation vulcanization crosslinking does not require the addition of vulcanizing agents and can be carried out at room temperature and pressure. Compared with traditional chemical vulcanization processes, electron beam radiation vulcanization crosslinking processes can improve the aging resistance of fluoroelastomer compositions and accelerate the vulcanization speed.

[0047] S5 secondary vulcanization crosslinking: subjecting the room temperature radiation crosslinked fluoroelastomer composition to secondary high temperature vulcanization to obtain a microporous fluoroelastomer composition.

[0048] The combination of room temperature radiation vulcanization cross-linking and conventional high temperature vulcanization cross-linking can significantly reduce the vulcanization time, obtain a stable microporous composition, and improve the mechanical properties of the product.

[0049] In one embodiment, the secondary vulcanization condition in S5 is 200-220° C., 0.5-4 hr.

[0050] In one embodiment, a vulcanizing agent and a cross-linking accelerator may be added in the pre-molding stage in step 1 to facilitate molding.

[0051] In step 1, 1-2 parts of a vulcanizing agent and 0.3-3 parts of an accelerator may also be added. The vulcanizing agent includes at least one of bisphenol AF, di-tert-butyl peroxide isopropylbenzene (BIPB), and dipentadienyl vulcanizing agent, and the accelerator is at least one of benzyl triphenylphosphine chloride (BPP accelerator) and triallyl isocyanurate (TAIC).

[0052] In one embodiment, the radiation vulcanization cross-linking in step S4 is performed at room temperature using a linear electron accelerator, and the radiation dose is 15-100 kGy.

[0053] The above method uses the process of "pre-vulcanization molding - physical foaming shaping - radiation vulcanization cross-linking - secondary vulcanization cross-linking" to prepare a high-strength, ozone-resistant microporous fluoroelastomer composition using supercritical carbon dioxide foaming and radiation vulcanization cross-linking. High pressure or supercritical fluid is used as a physical foaming agent to obtain a smaller cell size and a more uniform cell structure; and room temperature radiation vulcanization cross-linking and secondary high temperature vulcanization are used to shorten the vulcanization production time, stabilize the microporous structure, and thus ensure that the fluoroelastomer composition has strong ozone resistance.

[0054] A microporous fluoroelastomer composition is prepared by the above method.

[0055] Examples 1-4 S1, mixing fluoroelastomer, nucleating agent, vulcanizing agent, cross-linking accelerator and other fillers to obtain fluoroelastomer compound rubber.

[0056] 100 parts of fluoroelastomer (Daikin G-343 binary bisphenol vulcanization system premixed rubber, Mooney viscosity (ML1+100, 100°C) 39); the nucleating agent is silicon dioxide, 10 parts by weight; the vulcanizing agent is bisphenol AF vulcanizing agent, 1 part by weight; the cross-linking accelerator is BPP accelerator, 0.3 parts by weight; the filler is carbon black N990, 10 parts by weight; the acid absorber is MgO, 6 parts by weight.

[0057] S2, compression molding the fluoroelastomer compound to obtain a fluoroelastomer composition that is not microporous and not post-cured.

[0058] S3, place the non-microporous and non-secondary vulcanized fluoroelastomer composition in a molding mold, seal it in an autoclave, use high pressure or supercritical fluid to replace the air and increase the pressure, control the temperature and pressure in the autoclave, and after the high pressure or supercritical fluid reaches or approaches the dissolution equilibrium in the non-microporous and non-secondary vulcanized fluoroelastomer composition, stop heating and quickly release the pressure to allow the non-microporous and non-secondary vulcanized fluoroelastomer composition to expand in the molding mold, cool and shape to obtain a microporous but unvulcanized fluoroelastomer composition. The autoclave uses high-pressure CO2 fluid. The pressure control range of CO2 in the autoclave is 10 MPa, the temperature control range is 90 ℃, the pressure holding time is 5 hr, and the pressure is quickly released after the pressure is held, and the pressure release time is 5 s; the CO2 foaming multiple is about 6 times.

[0059] S4, the microvoided but not post-vulcanized fluoroelastomer composition is subjected to radiation vulcanization, and the radiation doses are 20 kGy, 40 kGy, 60 kGy, and 80 kGy, respectively.

[0060] S5, subjecting the cross-linked fluoroelastomer composition to secondary vulcanization cross-linking at a temperature of 200° C. for 2 hours to obtain a microporous fluoroelastomer composition.

[0061] The proportions of the components in Examples 1 to 4 are the same, and the difference lies in the different radiation doses.

[0062] Comparative Example 1 S1, mixing fluoroelastomer, nucleating agent, vulcanizing agent, cross-linking accelerator and other fillers to obtain fluoroelastomer compound rubber.

[0063] 100 parts of fluoroelastomer (Daikin G-343 binary bisphenol vulcanization system premixed rubber, Mooney viscosity (ML1+100, 100°C) 39); the nucleating agent is silicon dioxide, 10 parts by weight; the vulcanizing agent is bisphenol AF vulcanizing agent, 1 part by weight; the cross-linking accelerator is BPP accelerator, 0.3 parts by weight; the filler is carbon black N990, 10 parts by weight; the acid absorber is MgO, 6 parts by weight.

[0064] S2, molding the fluoroelastomer compound and performing a first vulcanization to obtain a fluoroelastomer composition that is not microporous and not secondarily vulcanized.

[0065] S3, placing the non-microporous and non-secondary-vulcanized fluoroelastomer composition in a molding mold, the CO2 pressure control range in the autoclave is 10 MPa, the temperature control range is 90 ° C, the pressure holding time is 5 hr, and the pressure is quickly released after pressure holding, and the pressure release time is 5 s; the CO2 foaming multiple is about 6 times.

[0066] S4, subjecting the microporous fluoroelastomer composition that has not been post-vulcanized to conventional high temperature vulcanization to achieve post-vulcanization, wherein the high temperature vulcanization temperature is 200° C. and the vulcanization time is 18 hours, to obtain a microporous fluoroelastomer composition.

[0067] The following instruments and equipment were used: Electronic universal testing machine: JPL-5000N, Jiangsu Tuoda Precision Testing Instrument Co., Ltd. Internal mixer: BL-6172-B, Guangdong Baolun Precision Testing Instrument Co., Ltd. Mixing mill: KL-9, Baihong Machinery (Shanghai) Co., Ltd. High-speed homogenizer: A30-Digital, Shanghai Ouhe Machinery Equipment Co., Ltd. Thermoforming machine: TYC-7-S-PCD, Dongyu (Ningbo) Hydraulic Industry Co., Ltd. Supercritical CO2 equipment: SFE-650M, Siangjia (Beijing) Biotechnology Co., Ltd. Precision bellows: Yiheng BPG-9106B, 250℃ Balance: AP125WD (Shimadzu) Density meter: FA2204C, Tianmei (China) Scientific Instrument Co., Ltd. Jet plasma cleaning machine: Triron 40, Shanghai Jiyi Technology Co., Ltd. The room temperature radiation uses a linear electron accelerator IS1024 model with a power of 24 kW and an electron energy of 10 MeV; the radiation dose is 15~100 kGy.

[0068] Examples and Comparative Examples Conditions and Results

[0069] The working conditions for O3 plasma resistance are ICP: 133.65 MHz; plasma; gas type is O2 / N2; flow ratio: 50 sccm; pressure (mt): 500; power (W): 800.

[0070] The enterprise standard is Q / SMS 001-2024 Test method for plasma etching resistance of perfluoroether rubber seals, which can be obtained through the National Standard Information Public Service Platform.

[0071] The prepared microporous fluoroelastomer composition can be applied to thermal insulation materials of nuclear power plants and has the following characteristics: 1) High hardness: Shore hardness is 27-32; 2) Resistance to ozone plasma etching: weight loss rate is 0.7-2.2%.

[0072] The CO2 foaming multiple or expansion ratio is defined as CO2 foaming multiple = density before foaming (density of unfoamed elastomer) / density after foaming (density of foamed rubber).

[0073] The radiation dose has a great influence on the performance of the elastomer composition, and the radiation effect is a competitive mechanism. When the rubber is irradiated, the intermolecular crosslinking reaction and the degradation reaction occur simultaneously, that is, on the one hand, the molecular weight of the network macromolecules formed by intermolecular crosslinking continues to increase; on the other hand, the radiation causes the chemical bonds to break and the relative molecular weight to decrease. It can be seen from the above table that when the radiation dose is less than 40 kGy, the crosslinking reaction plays a leading role; when the radiation dose is greater than 60 kGy, the degradation reaction plays a leading role. The radiation dose is an important parameter for determining the radiation vulcanization crosslinking process of the elastomer composition.

[0074] Compared with Example 1, the hardness and ozone plasma etching resistance of Example 2 are improved, and the cross-linking reaction plays a leading role at this time; when the degradation reaction plays a leading role, such as Example 4, the hardness and ozone plasma etching resistance are reduced.

[0075] The hardness and ozone plasma etching resistance of the fluoroelastomer composition prepared by the secondary high-temperature vulcanization of Examples 1 to 4 for only 2 hours are not inferior to those of the fluoroelastomer composition after high-temperature vulcanization for 18 hours in Comparative Example 1. The entire process time is greatly shortened, and the cost of high-temperature vulcanization is also reduced.

[0076] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a microporous fluoroelastomer composition, characterized in that: include: Step 1: Pre-vulcanization molding: 100 parts by weight of fluoroelastomer, 5-25 parts by weight of nucleating agent, 0-20 parts by weight of filler, and 0-10 parts by weight of acid absorbent are mixed to obtain a fluoroelastomer compound; Step 2: physical shaping: molding the fluoroelastomer compound to obtain a fluoroelastomer composition that is not microporous and not post-cured; Step 3: Foaming and shaping: placing the non-microporous and non-secondary-cured fluoroelastomer composition in a molding mold, using high pressure or supercritical fluid to make the non-microporous and non-secondary-cured fluoroelastomer composition reach a dissolution equilibrium with the molding mold, then rapidly reducing pressure and expanding, cooling and shaping to obtain a microporous but non-secondary-cured fluoroelastomer composition; Step 4: Radiation vulcanization and crosslinking: Radiation vulcanization and crosslinking the microvoided but not secondary vulcanized fluoroelastomer composition to obtain a crosslinked fluoroelastomer composition; Step 5: Secondary vulcanization and crosslinking: The crosslinked fluoroelastomer composition is subjected to secondary vulcanization to obtain a microporous fluoroelastomer composition.

2. The method for preparing a microporous fluoroelastomer composition according to claim 1, characterized in that: The radiation vulcanization cross-linking in step 4 is performed by using a linear electron accelerator at room temperature, and the radiation dose is 15-100 kGy.

3. The method for preparing the microporous fluoroelastomer composition according to claim 1, characterized in that: The fluoroelastomer is a copolymer formed by vinylidene fluoride, a vulcanization point monomer and at least one of the following monomers: tetrafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, and perfluorophenoxypropyl vinyl ether.

4. The method for preparing a microporous fluoroelastomer composition according to claim 1, characterized in that: The nucleating agent includes at least one of talc, calcium carbonate, calcium stearate, zinc stearate, sodium benzoate, magnesium oxide, silicon dioxide, boron nitride, and PTFE particles.

5. The method for preparing a microporous fluoroelastomer composition according to claim 1, characterized in that: The filler includes at least one of carbon nanotubes, carbon black, graphene, silicon dioxide and titanium dioxide.

6. The method for preparing a microporous fluoroelastomer composition according to claim 1, characterized in that: The acid absorber includes at least one of MaO, Ca(OH)2, ZnO and CaO.

7. The method for preparing a microporous fluoroelastomer composition according to claim 1, characterized in that: In step 1, 1 to 2 parts of a vulcanizing agent and 0.3 to 3 parts of an accelerator are also added, wherein the vulcanizing agent includes at least one of bisphenol AF, di-tert-butyl peroxide isopropylbenzene, and dipentadienyl vulcanizing agent, and the accelerator is at least one of benzyl triphenylphosphine chloride and triallyl isocyanurate.

8. The method for preparing a microporous fluoroelastomer composition according to claim 1, characterized in that: In step 2, the compression molding conditions are 8-10 MPa, 160-175° C., and 5-16 min.

9. The method for preparing a microporous fluoroelastomer composition according to claim 1, characterized in that: In step 3, the component of the high pressure or supercritical fluid is carbon dioxide or nitrogen, the pressure in the autoclave is 8-40 MPa, and the temperature is 60-140°C.

10. The method for preparing a microporous fluoroelastomer composition according to claim 1, characterized in that: In step 3, the rapid pressure relief and expansion time is 1 to 15 s.

11. The method for preparing a microporous fluoroelastomer composition according to claim 1, characterized in that: In step 5, the secondary vulcanization conditions are 200-220°C, 0.5-4 hr.

12. A microporous fluoroelastomer composition, characterized in that: The microporous fluoroelastomer composition is prepared by the method according to any one of claims 1-11.