Dissolving and recycling method for automobile safety airbag cloth PA66
By using an aqueous formic acid solution and a co-solvent combined with azeotropic distillation of 1,2-dichloroethane, the problems of nylon performance degradation and high solvent toxicity during the recycling process are solved, achieving efficient and environmentally friendly PA66 dissolution and recycling, which is suitable for the dissolution and recycling of automotive airbag fabric.
Patent Information
- Application Number
- CN202411235847.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies for recycling PA66 automotive airbag fabric suffer from issues such as decreased nylon performance and high solvent toxicity, making it difficult to achieve efficient and environmentally friendly dissolution and recycling.
Methanol is used as the main solvent, supplemented by co-solvents such as sodium benzoate, sodium salicylate, KCl, CaCl2, NaCl, MgCl2, etc. PA66 is dissolved in formic acid aqueous solution, and 1,2-dichloroethane is used as an azeotropic agent for solvent separation to improve solubility and recovery efficiency.
It effectively removes silicone rubber coatings without the use of strong alkalis, improves the solubility and recycling efficiency of PA66, reduces energy consumption, and is suitable for large-scale industrial application.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material recycling, and in particular to a dissolving and recycling method for automobile airbag fabric PA66. Background Art
[0002] The automobile airbag system is an active safety device widely used in automobiles. Its main function is to protect the safety of the occupants of the vehicle by rapidly inflating the airbag in the event of a collision, reducing or avoiding the damage to the human body caused by the collision. The airbag is usually made of high-strength nylon 66 (PA66) material as the base fabric, and then covered with a sealing resin layer on the surface to achieve waterproof / oil and airtight effects to form an airbag fabric, which is finally sewn into an airbag.
[0003] After the airbag is used, it needs to be recycled to prevent environmental pollution and waste of resources. The surface of the common airbag fabrics on the market is coated with silicone rubber or chloroprene rubber. These coatings are incompatible with PA66. If they are melt-granulated with PA66, defects will be formed in the recycled PA66, seriously affecting product performance. Therefore, in order to obtain high-grade recycled PA66, it is necessary to remove the silicone rubber coating on the surface of the airbag fabric as completely as possible.
[0004] The existing airbag recycling technologies mainly include physical and chemical methods. Among them, the physical method mainly breaks down the airbag cloth into smaller pieces by mechanical crushing, and then performs subsequent cleaning and physical melt granulation. The chemical method requires the use of specific solvents. The PA66 in the airbag cloth can be extracted by chemical dissolution and then physically melted and granulated. It can also be obtained by chemical degradation to obtain monomers or prepolymers for re-synthesis of PA66.
[0005] For example, Chinese patent CN115889427A describes a physical recycling method for discarded PA66 airbags, including manual impurity removal, cutting, soaking degumming, crushing and drying, melt granulation and other processes, and finally obtains PA66 resin. However, the degumming agent used in this patent requires the use of strong alkali, and the soaking time is as long as 72 hours. PA66 soaked in strong alkali for a long time will cause molecular chain scission, which is more prone to degradation and yellowing during high-temperature melt extrusion granulation, affecting the performance of the recycled PA66 product.
[0006] Chinese patent CN107739525A discloses a method of using solvent to dissolve and recycle airbag fabric PA66, and further preparing nylon modified materials for automobile bumpers through a physical blending process. However, the phenol-glacial acetic acid solution used in the patent is highly toxic and difficult to completely remove in subsequent steps, making it difficult to promote on an industrial scale. Summary of the invention
[0007] Aiming at the problems of decreased nylon performance and high solvent toxicity in the dissolution and recovery of PA66 airbag cloth, the present invention provides a dissolution and recovery method for safety airbag cloth, which uses methanol as a main solvent and a co-solvent as an auxiliary solvent to efficiently recover PA66, and realizes low-temperature recovery and reuse of the solvent, thereby effectively improving the recovery efficiency and the performance of the recovered PA66.
[0008] To achieve the above object, the technical solution adopted by the present invention is:
[0009] A dissolving and recycling method for automobile airbag fabric PA66 comprises the following steps:
[0010] Step 1, crushing and washing the recycled airbag cloth;
[0011] Step 2, placing the cleaned airbag in a mixed solvent of a formic acid aqueous solution and a co-solvent, stirring and dissolving to obtain a solution containing PA66;
[0012] Step 3, filtering the PA66 solution obtained after dissolution to remove undissolved silica gel, inorganic particle impurities, etc. in the solution to obtain a PA66 filtrate, and the filter used for filtration has a mesh size between 80 and 600, preferably 200 to 400.
[0013] Step 4, after filtering, precipitating the filtrate containing PA66 in water, and filtering to obtain a PA66 filter cake and a precipitate;
[0014] Step 5, crushing the PA66 filter cake, washing it with ethanol, and drying it to obtain the recovered PA66;
[0015] Step 6, adding zeolite and 1,2-dichloroethane to the precipitate, separating and recovering formic acid by azeotropic distillation for reuse.
[0016] The molecular chains of PA66 have strong hydrogen bond interactions, and the solubility in solvents such as formic acid is very low. The present invention uses a mixed solution of formic acid and water as a solvent, and inorganic ion compounds such as sodium benzoate, sodium salicylate, KCl, CaCl2, NaCl, MgCl2, etc. as co-solvents. The co-solvents can reduce the hydrogen bond interaction between PA66 molecules and increase the solubility of PA66 in formic acid, thereby improving the solvent recovery efficiency. At the same time, when the mixed solution of formic acid and water is reused, it is difficult to efficiently separate formic acid and water due to the wide range of the azeotropic ratio of formic acid and water. Adding 1,2-dichloroethane can more efficiently separate formic acid and water, thereby improving the reuse efficiency of the solvent. The processing time is short, the separation efficiency is high, and the recovered PA66 has good performance.
[0017] The water content of the formic acid aqueous solution is 2 to 50%, preferably 2 to 20%;
[0018] Preferably, the co-solvent includes one or more of sodium benzoate, sodium salicylate, p-aminobenzoic acid, urea, niacinamide, acetamide, KCl, CaCl2, NaCl, MgCl2, and sorbitol.
[0019] More preferably, the co-solvent is one or more of KCl, CaCl2, NaCl, and MgCl2. The co-solvent has better solubility in a mixed solvent of formic acid and water, and has a better solubility-promoting effect.
[0020] Preferably, the mass percentage of the co-solvent in the mixed solvent is 0.1% to 10. If the co-solvent content is too low, the solubilizing effect will not be achieved. If the co-solvent content is too high, the co-solvent will not be dissolved in the solvent, and the purity of the recovered PA66 will be affected. The mass content of the co-solvent can be further preferably 0.5 to 5%.
[0021] Preferably, the length and width of the airbag cloth after being broken in step 1 are within 10 cm, and further within 5 cm.
[0022] Preferably, the mass content of the airbag fabric in the mixed solvent in step 2 is between 5% and 40%. If the content of the airbag fabric is low, the dissolution efficiency is insufficient, and if the content is too high, the solvent loses fluidity. The mass content of the airbag fabric can be preferably 10% to 30%, and more preferably 10% to 20%.
[0023] Preferably, the stirring and dissolving temperature in step 2 is 50-70°C, and the dissolving time is 0.1-4h, and more preferably 0.5-1h.
[0024] When filtering the PA66 solution in step 3, the filter used for filtering has a mesh size between 80 and 600, preferably between 200 and 400;
[0025] In step 4, when the PA66 solution is precipitated, the volume ratio of the solution to water is 1:1-10, preferably 1:2-3.
[0026] The zeolite used in step 6 is natural zeolite after grinding, the particle size of the zeolite is less than 100 microns, and the amount of zeolite added is 1-5% of the weight of the precipitate; the volume ratio of 1,2-dichloroethane to the precipitate is 1:10-20.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The present invention can effectively remove the silicone rubber coating on the surface of the airbag cloth without using harmful substances such as strong alkali, so as to ensure the performance of the recycled PA66 product; using formic acid as a solvent and introducing a co-solvent can greatly increase the solubility of PA66 in the formic acid solvent and improve the recovery efficiency;
[0029] (2) The solvent used in the present invention can be recycled, and the recovery efficiency of the solvent can be improved by adding an azeotropic agent to the solvent, thereby reducing energy consumption, which is beneficial to energy conservation and emission reduction. Compared with traditional chemical recovery processes, the energy consumption is lower and it is more conducive to large-scale industrial promotion. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.
[0031] The raw materials used in the following specific embodiments are all purchased from the market, and the waste airbag cloth comes from the discarded safety airbags in the process of dismantling cars.
[0032] Example 1
[0033] Step 1: The recycled waste airbag cloth is crushed by a crusher, and the size of the crushed pieces is controlled within 10 cm in length and width; the crushed airbag cloth is added to a high-speed friction cleaning machine to remove surface dust and chemical substances adhering to the surface after the airbag is detonated;
[0034] Step 2, adding 100 parts of the cleaned airbag fabric into a solvent (the solvent is a mixed solvent of formic acid and water in a mass ratio of 80:20), then adding 0.5 parts of CaCl2 into the solvent, heating to 60°C and stirring to dissolve, the mass fraction of the airbag fabric in the solution is 15wt%, and the airbag fabric is completely dissolved after stirring for 1 to 2 hours;
[0035] Step 3, filtering the dissolved PA66 solution to remove impurities such as the adhesive layer remaining on the surface of the airbag cloth; slowly precipitating the PA66 filtrate into deionized water, with the volume ratio of the PA66 filtrate to the deionized water being 1:3; and filtering to obtain a PA66 filter cake and a precipitate containing formic acid and water;
[0036] Step 4: adding zeolite and 1,2-dichloroethane with a mass content of 3% of the precipitate to the precipitate, wherein the volume ratio of the precipitate to 1,2-dichloroethane is 20:1; performing intermittent azeotropic distillation at atmospheric pressure to separate formic acid, water and 1,2-dichloroethane solution, wherein the mass content of the formic acid obtained by distillation is about 81%, and the formic acid can be recycled as a good solvent for nylon.
[0037] Step 5, the PA66 filter cake is crushed into powder by a high-speed crusher, and then the powder is stirred and boiled with ethanol for 3 times, and dried in a blast drying oven to obtain PA66 powder, which is melt-granulated by a screw extruder to obtain recycled PA66 particles, and injection-molded to obtain corresponding specimens for performance testing.
[0038] Example 2
[0039] The difference from Example 1 is that when nylon is dissolved, the cosolvent is sorbitol.
[0040] Comparative Example 1
[0041] The difference from Example 1 is that the good solvent for nylon is a phenol / tetrachloroethane solution (the volume ratio of the two is 1 / 1). Since the boiling points of phenol and tetrachloroethane are relatively high, the filtrate obtained after filtration is difficult to be purified by distillation.
[0042] Comparative Example 2
[0043] The difference from Example 2 is that no co-solvent is added when the nylon is dissolved. When the nylon content is 15%, a viscous substance is formed, which loses good fluidity and is easy to quickly clog the filter screen during filtration and impurity removal, making it difficult to enter the next step.
[0044] Example 3
[0045] The difference from Example 1 is that when the nylon is dissolved, the co-solvent is MgCl2, and the amount used is 1 part relative to the mass of the airbag fabric.
[0046] Performance Testing
[0047] The PA66 recovered in Example 1-2 was prepared into test specimens, and the ash content, relative viscosity, IZOD notched impact, tensile strength, elongation at break, flexural strength, flexural modulus and other properties of PA66 were characterized according to ISO standards. See the data in Table 1 for details.
[0048] Table 1 Performance characterization data of recycled PA66 obtained in Examples 1-3
[0049] formula Example 1 Example 2 Example 3 Ash content (%) 0.12 0.21 0.36 Relative viscosity 3.26 3.23 3.21 <![CDATA[Izod impact strength (KJ / m 2 )]]> 6.8 6.5 6.5 Tensile strength(MPa) 81.2 79.3 80.6 Bending strength(MPa) 115.3 112.6 113.8 Flexural modulus (MPa) 2231.6 2156.3 2209.5
[0050] According to the data in Table 1, the impact strength of the high-value airbag cloth recycled PA66 material provided by the present invention is maintained at 5KJ / m 2 The above, tensile strength is higher than 70MPa, flexural strength is higher than 100MPa, flexural modulus is higher than 2GPa.
Claims
1. A dissolving and recycling method for automobile airbag fabric PA66, characterized in that: Includes steps: Step 1, crushing and washing the recycled airbag cloth; Step 2, placing the cleaned airbag in a mixed solvent of a formic acid aqueous solution and a co-solvent, stirring and dissolving, and then filtering to obtain a filtrate containing PA66; Step 3, after filtering, precipitating the filtrate containing PA66 in water to obtain a PA66 filter cake and a precipitate; Step 4, crushing the PA66 filter cake, washing it with ethanol, and drying it to obtain the recovered PA66; Step 5, adding zeolite and 1,2-dichloroethane to the precipitate, separating and recovering formic acid by azeotropic distillation for reuse.
2. The method for dissolving and recovering PA66, a fabric for automobile airbags, according to claim 1, characterized in that: The cosolvent includes one or more of sodium benzoate, sodium salicylate, p-aminobenzoic acid, urea, niacinamide, acetamide, CaCl2, MgCl2, and sorbitol.
3. The method for dissolving and recovering PA66, a fabric for automobile airbags, according to claim 1, characterized in that: The co-solvent is one or more of KCl, CaCl2, NaCl, and MgCl2.
4. The method for dissolving and recovering PA66, a fabric for automobile airbags, according to claim 1, characterized in that: The mass percentage of the co-solvent in the mixed solvent is 0.1-10%.
5. The method for dissolving and recovering PA66, a fabric for automobile airbags, according to claim 1, characterized in that: The length and width of the airbag cloth after being crushed in step 1 are within 10 cm.
6. The method for dissolving and recovering PA66, a fabric for automobile airbags, according to claim 1, characterized in that: In step 2, the mass content of the airbag fabric in the mixed solvent is 5-40%.
7. The method for dissolving and recovering PA66, a fabric for automobile airbags, according to claim 1, characterized in that: In step 2, the stirring and dissolving temperature is 50-70° C., and the dissolving time is 0.1-4 h.
8. The method for dissolving and recovering PA66 for automobile airbag fabric according to claim 1, characterized in that: In step 3, the volume ratio of the filtrate containing PA66 to water is 1:1-10.
9. The method for dissolving and recovering PA66, a fabric for automobile airbags, according to claim 1, characterized in that: The zeolite added in step 5 is natural zeolite with a particle size of less than 100 microns, and the amount of zeolite added is 1-5% of the weight of the precipitate; the volume ratio of 1,2-dichloroethane to the precipitate is 1:10-20.