Method for separating components of waste cotton-polyester blended fabric based on composite acid

Through the heating degradation and ultrasonic cleaning technology of the composite acid system, the problems of equipment corrosion, environmental pollution and high energy consumption in the separation of waste polyester and cotton blended textiles are solved, and efficient separation and recycling of polyester and cotton fibers are achieved, reducing costs and improving Environmentally friendly performance.

CN118930966AActive Publication Date: 2024-11-12FUZHOU UNIV

Patent Information

Application Number
CN202410997540.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The existing separation technology of waste polyester-cotton blended textiles has problems such as equipment corrosion, environmental pollution, high energy consumption, high cost and damage to fiber performance, making it difficult to achieve efficient separation with low cost and no secondary pollution.

Method used

Using a composite acid-based method, including placing the waste polyester and cotton blended fabric in a composite acid system of organic acid, inorganic acid and Lewis acid for heating and degradation, through ultrasonic cleaning and solid-liquid separation, recovery of polyester and cotton fibers respectively, and cooling Crystallization technology recycles organic acids and realizes recycling.

Benefits of technology

It realizes efficient and precise separation of polyester and cotton fiber, improves recycling rate and purity, reduces production costs, significantly improves environmental protection performance, and provides a new and economical and green way for the resource utilization of waste polyester and cotton blended textiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930966A_ABST
    Figure CN118930966A_ABST
Patent Text Reader

Abstract

The invention relates to a method for separating components of a waste cotton-polyester blended fabric based on composite acid. Through the synergistic effect of a composite acid system formed by combining organic acid, inorganic acid and Lewis acid, a hydrogen bond network in cellulose of the waste cotton-polyester blended fabric is effectively destroyed, cotton fibers are efficiently depolymerized, polyester fibers are released, and efficient and accurate separation of the waste cotton-polyester blended fabric is achieved. The separation efficiency is improved, the degradation selection specificity among the components is remarkably enhanced, high-purity recovery of the polyester and the cotton fibers is ensured, the original performance of the polyester and the cotton fibers can be reserved, and an effective means is provided for resource utilization of the waste polyester-cotton blended textiles. According to the method, the required acid amount is remarkably reduced, the treatment time is remarkably shortened, the recovery rate and purity of polyester and cotton fibers are effectively improved, the production cost is reduced, the environmental protection performance is remarkably improved, and an economic and green new way is provided for recycling of waste polyester-cotton blended textiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of recycling waste polyester-cotton fabrics, and more specifically to a method for separating components of waste polyester-cotton blended fabrics based on composite acid. Background Art

[0002] my country's textile industry is large in scale, with a complete industrial chain, rich resources and technological advantages, and has played an important supporting role in my country's economic development and employment. However, with the continuous increase in textile consumption, the number of discarded textiles continues to grow, and the environmental pollution and resource waste caused by them are becoming increasingly serious. Among waste textiles, the content of polyester components is the highest, accounting for about 80% of the total fiber. Since polyester is mostly found in polyester-cotton textiles and is difficult to degrade in the natural environment, the resource recycling of waste polyester-cotton blended textiles is of great significance.

[0003] At present, a variety of methods have been proposed for the separation and recycling of waste polyester-cotton blended textiles, such as ionic liquid dissolution, acid hydrothermal method, alkaline hydrolysis method, alcoholysis method, sulfuric acid-mechanical method, etc., but each method has its limitations. Some separation methods use strong acids or other chemical reagents, which may cause equipment corrosion and environmental pollution. For example, although phosphotungstic acid (HPW) is an easily recyclable heteropolyacid, its use still needs to be cautious to avoid secondary pollution. During the separation process, some methods may cause changes in the properties of cellulose or polyester. For example, after treatment with sulfuric acid-mechanical method, cracks and holes appeared on the surface of cotton fibers, the length and fineness were significantly reduced, and the mechanical properties of polyester fibers were significantly reduced, indicating that inappropriate separation process may affect the final application of recycled materials. In addition, the implementation of any separation technology is accompanied by energy consumption and possible cost issues, especially those methods that require high temperature, high pressure or specific chemical reagents, which may lead to higher operating costs and energy consumption. With the global emphasis on environmental protection and sustainable development, the development of simpler, more efficient, environmentally friendly and sustainable separation technology for waste polyester-cotton blended textiles is a very urgent and important research direction. Summary of the invention

[0004] Therefore, it is necessary to provide a method for separating the components of waste polyester-cotton blended fabrics based on composite acid, so as to use low-cost, secondary pollution-free composite acid to achieve efficient separation and recovery of polyester and cotton fibers in waste polyester-cotton blended fabrics through simple operation, and ensure that the structure and various properties of polyester and cotton fibers are not destroyed during the separation and recovery process. At the same time, the organic acid in the composite acid is effectively recovered for recycling, so as to minimize the cost of industrial-scale production practice.

[0005] To achieve the above object, the present invention provides a method for separating components of waste polyester-cotton blended fabrics based on composite acid, comprising the following steps:

[0006] The pre-treated waste polyester-cotton blended fabric is placed in a composite acid system, wherein the composite acid system includes an organic acid, an inorganic acid and a Lewis acid, and heated and degraded to obtain a reacted polyester-cotton mixture;

[0007] The polyester-cotton mixture after the reaction is ultrasonically cleaned;

[0008] Solid-liquid separation, recovery of polyester and cotton fibers respectively.

[0009] Waste polyester-cotton blended fabrics that have been pre-treated by crushing, washing, drying and other steps are mixed with a composite acid solution containing a certain concentration of organic acid, inorganic acid and Lewis acid, and placed in a normal pressure container for heating and degradation. Organic acid is the main solvent for separating the components of waste polyester-cotton blended textiles. Due to its weak acidity, the hydrogen ions generated by ionization have weak damage to the glycosidic bonds, and mainly attack the amorphous region of cellulose, ensuring the integrity of cotton fibers. The addition of Lewis acid can promote the ring opening of functional groups on the fiber surface, penetrate into the interior of cellulose to attack and destroy hydrogen bonds, further destroy hydrogen bonds and disperse cellulose macromolecular chains through unsaturated hydrated ions, and help cotton fibers peel off from the polyester surface. Inorganic acid has strong oxidizing and catalytic effects, and the use of appropriate amounts can improve the separation efficiency of the reaction system. In addition, organic acid has little effect on the chemical stability and mechanical properties of fibers, and usually has strong lipophilicity. In the process of polyester-cotton separation, it can simultaneously remove grease and other pollutants on the surface of the fabric. The synergistic effect of these three different types of acids can enhance each other and work together on cellulose, effectively destroying its internal hydrogen bond network and reducing the amount of acid or treatment time required. The polyester and cotton fibers in the waste polyester-cotton blended fabrics are initially separated during the heating degradation; after the reaction is completed, hot water is added to terminate the reaction. Next, the solution mixture system is placed in an ultrasonic cleaning device to deeply clean the polyester and cotton fibers in the solution mixture system; then the polyester and cotton fibers are recovered separately by filtration and separation under vacuum; not only does it improve the separation efficiency, but it also helps to retain the original properties of polyester and cotton fibers, ensuring the secondary utilization performance of the recycled polyester, and providing an effective means for the resource utilization of waste polyester-cotton blended textiles. For the remaining filtrate after filtration, the organic acid solvent in the composite acid is recovered by cooling crystallization technology. The recovered organic acid solvent can continue to be used in the new waste polyester-cotton blended textile recycling process to achieve resource recycling.

[0010] Preferably, in the composite acid system, the mass concentration of the organic acid is 60-80wt%, the mass concentration of the inorganic acid is 1-5wt%, the mass concentration of the Lewis acid is 1-5wt%, and the balance is deionized water.

[0011] Preferably, the organic acid is one of oxalic acid, p-toluenesulfonic acid, malic acid, acetic acid and citric acid, the inorganic acid is one of sulfuric acid, hydrochloric acid and phosphoric acid, and the Lewis acid is aluminum chloride or zinc dichloride tetrahydrate.

[0012] Preferably, the organic acid is oxalic acid. Low-cost oxalic acid can be produced industrially from plant resources. It is naturally abundant, biodegradable, non-volatile, and easy to recycle, making it a sustainable reagent.

[0013] Preferably, the temperature of the heating degradation is 95-115° C. and the time is 1-3 hours. By optimizing the precise control of the temperature, time and other parameters of the heating degradation, the separation effect is improved and the energy consumption and cost are reduced.

[0014] Preferably, the ultrasonic cleaning temperature is 50-70°C and the time is 10-30 minutes. Before ultrasonic cleaning, 100°C hot water is added to the mixed system after the insulation to terminate the degradation reaction. By optimizing the temperature, time and other conditions of ultrasonic cleaning, dirt and grease on the fiber surface are removed, and the separation effect is further improved.

[0015] Preferably, the cotton fiber content in the waste polyester-cotton blended fabric is 1-99wt%.

[0016] Preferably, the solid-liquid separation comprises the following steps: preliminary filtering the mixed solution after ultrasonic cleaning to obtain recovered polyester fibers and preliminary filtrate; and filtering and recovering the preliminary filtrate again by vacuum suction drainage to obtain cotton fibers.

[0017] Preferably, the solid-liquid mass ratio of the pre-treated waste polyester-cotton blended fabric to the composite acid system is 1:10-100.

[0018] Preferably, the method further comprises the following steps: recovering the filtrate after the solid-liquid separation to obtain a mixed solution containing organic acid crystals, cooling the mixed solution in an environment of 2-4°C for 16-24h to obtain fully crystallized organic acid, further filtering to obtain wet organic acid crystals, heating the mixed solution in a vacuum environment to obtain dry, high-purity organic acid crystals.

[0019] Different from the prior art, the above technical solution effectively destroys the hydrogen bond network inside the cellulose of waste polyester-cotton blended fabrics through the synergistic effect of the composite acid system of organic acid, inorganic acid and Lewis acid, efficiently depolymerizes cotton fibers, releases polyester fibers, and realizes efficient and accurate separation of waste polyester-cotton blended fabrics. The above technical solution not only improves the separation efficiency, but also significantly enhances the degradation selection specificity between components, ensures the high-purity recovery of polyester and cotton fibers, and helps to retain the original properties of polyester and cotton fibers, ensures the secondary utilization performance of recycled polyester, and provides an effective means for the resource utilization of waste polyester-cotton blended textiles. The present invention significantly reduces the required amount of acid and processing time, effectively improves the recovery rate and purity of polyester and cotton fibers, reduces production costs, and significantly improves environmental protection performance, providing an economical and green new way for the recycling and reuse of waste polyester-cotton blended textiles. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A scanning electron microscope image of waste polyester-cotton blended textiles used in a specific embodiment of the present invention;

[0021] Figure 2 This is a scanning electron microscope image of a polyester fiber assembly obtained after the reaction by the method of the present invention;

[0022] Figure 3 is a scanning electron microscope image of cotton fibers obtained after the reaction according to the method of the present invention;

[0023] Figure 4 This is a comparison chart of Fourier transform infrared spectroscopy (FTIR) analysis of polyester fiber before and after the reaction;

[0024] Figure 5 The comparison diagram of Fourier transform infrared spectroscopy (FTIR) analysis of cotton fiber before and after reaction;

[0025] Figure 6 It is a Fourier transform infrared spectroscopy (FTIR) analysis comparison diagram of unreacted oxalic acid and recycled oxalic acid recycled 1 to 5 times respectively;

[0026] Figure 7 This is a comparison chart of cotton fibers recovered by sulfuric acid separation and cotton fibers recovered by composite acid separation. DETAILED DESCRIPTION

[0027] In order to explain the technical content, structural features, achieved objectives and effects of the technical solution in detail, the following is a detailed description in conjunction with specific embodiments and accompanying drawings.

[0028] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.

[0029] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.

[0030] In the description of this application, the term "and / or" is an expression used to describe the logical relationship between objects, indicating that three relationships may exist, for example, A and / or B, which means: A exists, B exists, and A and B exist at the same time. In addition, the character " / " in this article generally indicates that the objects before and after are in an "or" logical relationship.

[0031] In the present application, terms such as “first” and “second” are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship of quantity, priority or sequence between these entities or operations.

[0032] Without further limitations, in this application, the words "include", "comprises", "has" or other similar expressions used in the sentences are intended to cover non-exclusive inclusion. These expressions do not exclude the presence of additional elements in the process, method or product including the elements, so that the process, method or product including a series of elements may include not only those limited elements, but also other elements not explicitly listed, or also include elements inherent to such process, method or product.

[0033] Similar to the understanding in the Patent Examination Guidelines, in this application, expressions such as "greater than", "less than", "exceed" and the like are understood to exclude the number itself; expressions such as "above", "below", "within" and the like are understood to include the number itself. In addition, in the description of the embodiments of this application, "multiple" means more than two (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups", "multiple times", etc., unless otherwise clearly and specifically limited.

[0034] In the description of the embodiments of the present application, space-related expressions used, such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "vertical", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicate the orientation or position relationship based on the orientation or position relationship shown in the specific embodiments or drawings, and are only for the convenience of describing the specific embodiments of the present application or facilitating the reader's understanding, and do not indicate or imply that the referred device or component must have a specific position, a specific orientation, or be constructed or operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.

[0035] Unless otherwise expressly specified or limited, in the description of the embodiments of the present application, the terms such as "install", "connect", "connect", "fix", "set", etc. used should be understood in a broad sense. For example, the "connection" can be a fixed connection, a detachable connection, or an integrated setting; it can be a mechanical connection, an electrical connection, or a communication connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. For technicians in the technical field to which the present application belongs, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0036] The various instruments, equipment, raw materials or reagents used in the specific embodiments of the present invention are not limited in terms of their sources, and are all conventional products that can be purchased through regular commercial channels, or can be prepared according to conventional methods well known to those skilled in the art. The waste polyester-cotton blended raw materials used in the following examples are waste fabrics recycled from factories, and the chemical reagents used in the following examples are commercially available products and are analytically pure unless otherwise specified. The operations or instruments used in the following examples are common operations or instruments in the art unless otherwise specified. The proportions, ratios, contents, etc. described in the following examples are weight ratios unless otherwise specified, and the recovery rate refers to the ratio of the polyester (or cotton fiber) collected after separation to the polyester (or cotton fiber) content in the untreated waste polyester-cotton textiles.

[0037] The calculation of polyester purity is as follows: the recycled polyester fiber is passed through the national standard GB / T 2910.11-2009 "Quantitative Chemical Analysis of Textiles Part 11: Mixture of Cellulose Fibers and Polyester Fibers (Sulfuric Acid Method)", and the cellulose fiber is dissolved and removed from the mixture of known dry mass with sulfuric acid, and the residue is collected, washed, dried and weighed; the corrected mass is used to calculate its percentage of the dry mass of the mixture. The polyester fiber purity is calculated by the ratio of the polyester fiber mass obtained by the reaction to the polyester fiber mass before the reaction.

[0038] The loss rate of polyester is obtained by calculating the difference between the polyester mass after separation and the polyester content in the original fabric, and the ratio of the difference to the mass of the original fabric. The loss rate of cotton fiber is obtained by calculating the difference between the cotton fiber mass after separation and the cotton fiber content in the original fabric, and the ratio of the difference to the mass of the original fabric.

[0039] The test and calculation methods of intrinsic viscosity and degree of polymerization refer to GB / T 14190-2017 "Test method for fiber-grade polyester (PET) chips". The sample was dissolved in a mixture of phenol / tetrachloroethane (mass ratio 50:50) at 90°C, and the efflux time of the solvent at 25°C and the PET solution with a concentration of 0.005 g / ml was measured using an Ubbelohde viscometer. The intrinsic viscosity was calculated based on the measured efflux time and the solution concentration of the sample. The degree of polymerization was obtained by the ratio of the average molecular weight of the polymer to the molecular weight of the polymerization unit.

[0040] In addition, the method of the present invention does not involve the use of more harmful chemicals, nor does it require the use of large amounts of more expensive solvents. Instead, water is used as the reaction medium, and the acid solution used is easily recyclable and reusable, which helps to reduce fiber recycling costs, improve production efficiency, and achieve truly "green and environmentally friendly" recycling and reuse of polyester-cotton blended textiles.

[0041] Example 1

[0042] Take a certain amount of waste polyester-cotton blended fabric raw material with a cotton content of 32% and a polyester content of 68%, wash it with water, cut or crush it into blocks of about 1.0000±0.0002g, put it in an oven to dry it, and then put it in a dryer to dry it to constant weight to obtain the waste polyester-cotton blended fabric after pretreatment. Take it out, use a weighing bottle to weigh and record the mass of the waste polyester-cotton blended fabric after pretreatment, put it into a composite acid system solution composed of 5wt% oxalic acid, 5wt% sulfuric acid and 5wt% aluminum chloride, and the remainder is deionized water, and the mass ratio of the waste polyester-cotton blended fabric after pretreatment to the composite acid system solution is 1:10, set the temperature of the digital display constant temperature oil bath pot to 105℃, and the reaction time is 3h, in which the degradation reaction of cotton fibers in the waste polyester-cotton blended fabric is completed. After the reaction is completed, add enough 100℃ hot water to stop the reaction. The mixed solution after the reaction is stopped is placed in an ultrasonic cleaning device and ultrasonic deep cleaning is performed at 60℃ for 20min. Then, the polyester fiber is initially filtered to obtain the recovered polyester fiber, which is washed with cold water several times, and the initial filtrate is drained through the filter membrane under vacuum suction conditions, and filtered again to obtain the cotton fiber. Finally, the recovered polyester fiber and cotton fiber are dried in an oven for 4-16 hours, and then placed in a dryer to cool and dry to constant weight, and taken out and weighed within 2 minutes.

[0043] Example 2

[0044] The difference from Example 1 is that the added composite acid system solution contains 60wt% oxalic acid, 5wt% sulfuric acid and 5wt% aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0045] Example 3

[0046] The difference from Example 1 is that the added composite acid system solution contains 65wt% oxalic acid, 5wt% sulfuric acid and 5wt% aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0047] Example 4

[0048] The difference from Example 1 is that the added composite acid system solution contains 70 wt % oxalic acid, 5 wt % sulfuric acid and 5 wt % aluminum chloride, and the balance is deionized water. The other operation steps and parameters are the same as those in Example 1.

[0049] Example 5

[0050] The difference from Example 1 is that the added composite acid system solution contains 80 wt % oxalic acid, 5 wt % sulfuric acid and 5 wt % aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0051] The recovery rates of polyester and cotton fibers recovered in Examples 1 to 5 were calculated according to the ratio of recovery rate = polyester (or cotton fiber) collected after separation / polyester (or cotton fiber) content in untreated waste polyester-cotton textiles, and the recovery rates of polyester and cotton fibers were used as evaluation indicators. It was found that the separation effect of the composite acid system solution containing 70wt% oxalic acid in the mixed solution system was the best, the recovery rate of separated polyester was above 99%, and the recovery rate of cotton fibers could reach up to 94.01%. The loss rates of the recovered polyester fiber and cotton fiber are calculated according to the loss rate = the ratio of the difference between the polyester (or cotton fiber) collected after separation / the polyester (or cotton fiber) content in the untreated waste polyester-cotton textiles and the polyester (or cotton fiber) content in the untreated waste polyester-cotton textiles. The purity of the polyester fiber is calculated by the ratio of the mass of the polyester fiber obtained by reacting the recovered polyester fiber with reference to GB / T2910.11-2009 "Quantitative Chemical Analysis of Textiles Part 11: Mixture of Cellulose and Polyester Fibers (Sulfuric Acid Method)" to the mass of the polyester fiber before the reaction. The polyester purity is 100%, the polyester mass loss rate is less than 1%, and the cotton fiber mass loss rate is less than 5%.

[0052] Example 6

[0053] The difference from Example 1 is that the added composite acid system solution contains 70 wt % oxalic acid, 1 wt % sulfuric acid and 5 wt % aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0054] Example 7

[0055] The difference from Example 1 is that the added composite acid system solution contains 70 wt % oxalic acid, 3 wt % sulfuric acid and 5 wt % aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0056] Example 8

[0057] The difference from Example 1 is that the added composite acid system solution contains 70 wt % oxalic acid, 3 wt % sulfuric acid and 5 wt % aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0058] The recovery rates of polyester and cotton fibers recovered in Examples 6 to 8 were calculated according to the ratio of recovery rate = polyester (or cotton fiber) collected after separation / polyester (or cotton fiber) content in untreated waste polyester-cotton textiles, and the recovery rates of polyester and cotton fibers were used as evaluation indicators. It was found that the separation effect of the composite acid system solution containing 3wt% sulfuric acid in the mixed solution system was the best, and the recovery rate of separated polyester was above 99%, and the recovery rate of cotton fibers could reach up to 94.89%. The polyester fiber purity was calculated by referring to the ratio of the polyester fiber mass obtained by reaction with reference to GB / T 2910.11-2009 "Quantitative Chemical Analysis of Textiles Part 11: Mixtures of Cellulose Fibers and Polyester Fibers (Sulfuric Acid Method)" to the polyester fiber mass before reaction. The polyester purity was 100%, the polyester mass loss rate was less than 1%, and the cotton fiber mass loss rate was less than 5%.

[0059] Example 9

[0060] The difference from Example 1 is that the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 1wt% aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0061] Example 10

[0062] The difference from Example 1 is that the added composite acid system solution contains 70 wt % oxalic acid, 3 wt % sulfuric acid and 3 wt % aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0063] Embodiment 11

[0064] The difference from Example 1 is that the added composite acid system solution contains 70 wt % oxalic acid, 3 wt % sulfuric acid and 4 wt % aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0065] Example 12

[0066] The difference from Example 1 is that the added composite acid system solution contains 70 wt % oxalic acid, 3 wt % sulfuric acid and 5 wt % aluminum chloride, and the balance is deionized water. The other operating steps and parameters are the same as those in Example 1.

[0067] The recovery rates of polyester and cotton fibers recovered in Examples 9 to 12 were calculated according to the ratio of recovery rate = polyester (or cotton fiber) collected after separation / polyester (or cotton fiber) content in untreated waste polyester-cotton textiles, and the recovery rates of polyester and cotton fibers were used as evaluation indicators. It was found that the separation effect of the composite acid system solution containing 4wt% aluminum chloride in the mixed solution system was the best, and the recovery rate of separated polyester was above 99%, and the recovery rate of cotton fiber could reach up to 95.05%. The polyester fiber purity was calculated by referring to the ratio of the polyester fiber mass obtained by reaction with reference to GB / T 2910.11-2009 "Quantitative Chemical Analysis of Textiles Part 11: Mixtures of Cellulose Fibers and Polyester Fibers (Sulfuric Acid Method)" to the polyester fiber mass before reaction. The polyester purity was 100%, the polyester mass loss rate was less than 1%, and the cotton fiber mass loss rate was less than 5%.

[0068] Example 13

[0069] The difference from Example 1 is that the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water. The temperature of the digital display constant temperature oil bath is set to 95°C, and the other operating steps and parameters are carried out according to Example 1.

[0070] Embodiment 14

[0071] The difference from Example 13 is that the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water. The temperature of the digital display constant temperature oil bath is set to 97°C, and the other operating steps and parameters are carried out according to Example 1.

[0072] Embodiment 15

[0073] The difference from Example 1 is that the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water. The temperature of the digital display constant temperature oil bath is set to 100°C, and the other operating steps and parameters are carried out according to Example 1.

[0074] Example 16

[0075] The difference from Example 1 is that the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water. The temperature of the digital display constant temperature oil bath is set to 110°C, and the other operating steps and parameters are carried out according to Example 1.

[0076] Embodiment 17

[0077] The difference from Example 1 is that the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water. The temperature of the digital display constant temperature oil bath is set to 115°C, and the other operating steps and parameters are carried out according to Example 1.

[0078] The recovery rates of polyester and cotton fibers recovered in Examples 13 to 17 were calculated according to the ratio of recovery rate = polyester (or cotton fiber) collected after separation / polyester (or cotton fiber) content in untreated waste polyester-cotton textiles, and the recovery rates of polyester and cotton fibers were used as evaluation indicators. It was found that the separation effect was best when the heating degradation temperature was 97°C, the recovery rate of separated polyester was above 99%, and the recovery rate of cotton fiber could reach up to 97.22%. The polyester fiber purity was calculated by referring to the ratio of the mass of polyester fiber obtained by reaction with reference to GB / T 2910.11-2009 "Quantitative Chemical Analysis of Textiles Part 11: Mixtures of Cellulose Fibers and Polyester Fibers (Sulfuric Acid Method)" to the mass of polyester fiber before reaction. The polyester purity was 100%, the polyester mass loss rate was less than 1%, and the cotton mass loss rate was less than 5%.

[0079] Embodiment 18

[0080] The difference from Example 1 is that the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water. The temperature of the digital display constant temperature oil bath is set to 97°C, the reaction time is 1h, and the other operating steps and parameters are carried out according to Example 1.

[0081] Embodiment 19

[0082] The difference from Example 1 is that the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water. The temperature of the digital constant temperature oil bath is set to 97°C, the reaction time is 2h, and the other operating steps and parameters are carried out according to Example 1.

[0083] Embodiment 20

[0084] The difference from Example 1 is that the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water. The temperature of the digital display constant temperature oil bath is set to 97°C, the reaction time is 3h, and the other operating steps and parameters are carried out according to Example 1.

[0085] The recovery rates of polyester and cotton fibers recovered in Example 18-Example 20 were calculated according to the ratio of recovery rate = polyester (or cotton fiber) collected after separation / polyester (or cotton fiber) content in untreated waste polyester-cotton textiles, and the recovery rates of polyester and cotton fibers were used as evaluation indicators. It was found that the separation effect was best when the heating degradation time was 1 hour, and the recovery rate of separated polyester was above 99%, and the recovery rate of cotton fiber could reach up to 96.53%. The polyester fiber purity was calculated by referring to the ratio of the mass of polyester fiber obtained by reaction with reference to GB / T 2910.11-2009 "Quantitative Chemical Analysis of Textiles Part 11: Mixture of Cellulose Fibers and Polyester Fibers (Sulfuric Acid Method)" to the mass of polyester fiber before reaction. The polyester purity was 100%, the polyester mass loss rate was less than 1%, and the cotton fiber mass loss rate was less than 5%.

[0086] Embodiment 21

[0087] The difference from Example 1 is that the cotton fiber content in the waste polyester-cotton blended textile raw material used is 1wt%, the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water, the temperature of the digital display constant temperature oil bath is set to 97°C, the reaction time is 1h, and the other operating steps and parameters are carried out according to Example 1.

[0088] Embodiment 22

[0089] The difference from Example 1 is that the cotton fiber content in the waste polyester-cotton blended textile raw material used is 20wt%, the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water, the temperature of the digital display constant temperature oil bath is set to 97°C, the reaction time is 1h, and the other operating steps and parameters are carried out according to Example 1.

[0090] Embodiment 23

[0091] The difference from Example 1 is that the cotton fiber content in the waste polyester-cotton blended textile raw material used is 50wt%, the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water, the temperature of the digital display constant temperature oil bath is set to 97°C, the reaction time is 1h, and the other operating steps and parameters are carried out according to Example 1.

[0092] Embodiment 24

[0093] The difference from Example 1 is that the cotton fiber content in the waste polyester-cotton blended textile raw material used is 80wt%, the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water, the temperature of the digital display constant temperature oil bath is set to 97°C, the reaction time is 1h, and the other operating steps and parameters are carried out according to Example 1.

[0094] Embodiment 25

[0095] The difference from Example 1 is that the cotton fiber content in the waste polyester-cotton blended textile raw material used is 99wt%, the added composite acid system solution contains 70wt% oxalic acid, 3wt% sulfuric acid and 4wt% aluminum chloride, and the balance is deionized water, the temperature of the digital display constant temperature oil bath is set to 97°C, the reaction time is 1h, and the other operating steps and parameters are carried out according to Example 1.

[0096] The recovery rates of polyester and cotton fibers recovered in Example 21-Example 25 were calculated according to the ratio of recovery rate = polyester (or cotton fiber) collected after separation / polyester (or cotton fiber) content in untreated waste polyester-cotton textiles, and the recovery rates of polyester and cotton fibers were used as evaluation indicators. It was found that for fabrics with a cotton fiber content of 1-99wt% in polyester-cotton blended textiles, the method of the present invention achieved complete separation of polyester and cotton fibers, and the recovery rate of separated polyester was above 99%, and the recovery rate of cotton fibers could reach up to 96.53%. The polyester fiber purity was calculated by referring to the ratio of the polyester fiber mass obtained by reaction with reference to GB / T2910.11-2009 "Quantitative Chemical Analysis of Textiles Part 11: Mixtures of Cellulose Fibers and Polyester Fibers (Sulfuric Acid Method)" to the polyester fiber mass before reaction. The polyester purity was 100%, the polyester mass loss rate was less than 1%, and the cotton fiber mass loss rate was less than 5%.

[0097] From the above embodiments, it can be seen that the preferred process for separating the two components of waste polyester-cotton blended textiles based on composite acid of the present invention is: the waste polyester-cotton blended textiles are heated and degraded by a composite acid solution composed of 70% oxalic acid, 3% sulfuric acid and 4% aluminum chloride. The reaction temperature of the heating degradation is preferably 97°C, and the reaction time is preferably 1h. The cotton fiber content of the waste polyester-cotton textiles treated by the present invention is 1%-99%, that is, it is suitable for most polyester-cotton blended textiles.

[0098] The polyester and cotton fibers separated and recovered in Example 22 were tested by Fourier transform infrared spectroscopy (FTIR) and X-ray diffractometer (XRD). Figure 1 Scanning electron microscope image of untreated waste polyester-cotton textiles, Figure 2Scanning electron micrograph of the polyester fiber aggregate obtained after separation and recovery Figure 3 The scanning electron microscope image of the cotton fiber obtained after separation and recovery shows that the polyester component and cotton fiber component in the treated waste polyester-cotton textiles have been effectively separated, and the presence of cotton fiber can no longer be observed in the separated polyester ( Figure 2 ), the polyester and cotton fibers on the surface have been completely separated, and the surface of the polyester fibers is still smooth and undamaged; the cotton fibers are completely peeled off from the intertwined state with the polyester, and the separated cotton fibers are broken into curved fibers of different sizes ( Figure 3 ).

[0099] See also Figure 4 The Fourier transform infrared spectroscopy (FTIR) analysis comparison diagram of the polyester fiber before and after the reaction shows that the FTIR spectrum shape of the polyester fiber obtained by the composite acid treatment is consistent with that of the pure polyester fiber (pure polyester fiber fabric is 100% polyester fabric, provided by Fujian Huafeng New Materials Co., Ltd.), and no new peaks appear, indicating that the polyester fiber maintains its original chemical structure after the composite acid treatment. Pure polyester fiber is 100% polyester fabric, provided by Fujian Huafeng New Materials Co., Ltd.

[0100] See also Figure 5 The Fourier transform infrared spectroscopy (FTIR) analysis comparison of cotton fibers before and after the reaction is shown in the figure. It can be seen that compared with the untreated pure cotton fabric, the cotton fiber product treated with the composite acid solution has a wavelength of 1630 cm -1 An obvious carboxyl absorption peak appeared at the bottom, indicating that the separated product contained carboxyl groups, proving that the cotton fiber was hydrolyzed and oxidized to oxidized cellulose containing carboxyl groups.

[0101] Therefore, the chemical structure of the polyester separated from the waste polyester-cotton blended fabric is consistent with that of the pure polyester fiber (reference), and the chemical structure of the separated cotton fiber is basically consistent with that of the pure cotton fabric.

[0102] Referring to GB / T 14190-2017 "Test Method for Fiber-Grade Polyester (PET) Chips", the sample was dissolved in a mixture of phenol / tetrachloroethane (mass ratio 50:50) at 90°C, and the efflux time of the solvent at 25°C and the PET solution with a concentration of 0.005g / ml was measured using an Ubbelohde viscometer. The intrinsic viscosity was calculated based on the measured efflux time and the solution concentration of the sample, and the degree of polymerization was obtained by the ratio of the average molecular weight of the polymer to the molecular weight of the polymerization unit. The intrinsic viscosity and degree of polymerization of the polyester fiber before and after treatment were tested, and the results showed that the intrinsic viscosity and degree of polymerization of the polyester fiber before and after treatment changed little, with the intrinsic viscosity being 0.66dl / g and 0.70dl / g, respectively, the degree of polymerization before treatment being 98, and the degree of polymerization of the polyester fiber after treatment being 106. The separated polyester still showed excellent mechanical properties after the test.

[0103] Embodiment 26

[0104] The filtrate containing oxalic acid crystals after filtering and separating the polyester fiber and cotton fiber in Example 1 is placed in an environment of 2-4°C and cooled for 16-24h to ensure that the oxalic acid can fully crystallize; after the oxalic acid crystals are completed, filter paper or filter is used to leave the oxalic acid crystals on the filter, and the aqueous solution flows out through the filter. The oxalic acid crystals obtained by filtration also contain a certain amount of moisture or other impurities. They are placed in a vacuum environment and heated to evaporate the moisture and other volatile substances in the oxalic acid crystals to obtain 30.4g of dry, high-purity oxalic acid crystals. It can be observed that the oxalic acid obtained is not much different from the oxalic acid that does not participate in the reaction, and still presents a white crystalline state. The oxalic acid is recovered and recycled 5 times in the composite acid system solution to participate in the polyester-cotton recovery and separation of waste polyester-cotton blended fabrics. A total of 32g of fresh oxalic acid was initially used. The recovery rate was calculated to show that the total amount of oxalic acid gradually decreased in each consumption as the number of cycles increased. However, after 5 cycles, the total amount of oxalic acid recovered was still 26.5g, and the total recovery rate of 5 cycles was as high as 82.8%. The oxalic acid recovery rate in a single cycle is higher than 95%. Figure 6 The Fourier transform infrared spectroscopy (FTIR) analysis comparison diagram of the unreacted oxalic acid and the recycled oxalic acid respectively recycled 1 to 5 times shows that the chemical structure of the oxalic acid remains unchanged after the oxalic acid is recycled and repeated 4 times, and its chemical composition is still oxalic acid, and no other obvious impurities are generated. It can be seen that the organic acid solvent used in the present invention can be recycled for many times, and the pollution to the environment caused by the discharge of chemicals can be reduced while ensuring the separation effect.

[0105] Comparative Example 1

[0106] Take a certain amount of waste polyester-cotton blended raw materials, cut them into blocks of about 1.0000±0.0002g, put them in an oven for 4-16h, take them out, and put them in a dryer to dry to constant weight. Add 350ml of concentrated sulfuric acid (ρ=1.84g / ml) to 150ml of water, and add water to 500ml after the solution cools to room temperature. Weigh 15ml of concentrated ammonia water and add 187.5ml of water. Prepare 75% sulfuric acid solution and dilute ammonia solution. Take out the sample pretreated in the dryer, weigh it with a weighing bottle and record the mass after drying, put it in a conical flask, add 200mL of the prepared 75% sulfuric acid solution for each gram of sample, plug it with a glass stopper, shake the flask to fully wet the sample, put the flask in a water bath thermostat and keep it at 50℃±5℃ for 1h, and shake it every 10min. After the reaction is completed, filter the reaction mixture into a glass sand core crucible, vacuum suction and drain, and then add a small amount of sulfuric acid to clean the flask. Drain by vacuum suction, add new sulfuric acid solution to the crucible to clean the residue, drain by gravity for at least 1 minute, then use vacuum suction. Wash with cold water several times, neutralize with dilute ammonia twice, and then wash with cold water. Drain by gravity first and then by suction each time. Finally, put the crucible and residue into the oven to dry for 4-16 hours, move to the dryer to cool and dry to constant weight, take out and weigh within 2 minutes, and obtain 0.6701g of polyester fabric. Please refer to Figure 7 A comparison chart of the cotton fibers recovered by separation with sulfuric acid and the cotton fibers recovered by separation with the composite acid shows that, compared with Example 1, the cotton fibers in the fabric treated with the comparative example were over-hydrolyzed, the fiber structure was severely damaged, and the cotton fibers could not be effectively recovered. This proves that the composite acid solution is more effective in separating the two components in waste polyester-cotton blended textiles and recycling polyester fibers and cotton fibers with higher recovery rates.

[0107] In summary, the component separation method of waste polyester-cotton blended textiles of the present invention has a simple and efficient process, low cost, no environmental pollution, and can be recycled. The polyester recovery rate in waste polyester-cotton blended textiles reaches more than 99%, the purity is 100%, and the polyester mass loss rate is less than 1%; the cotton fiber recovery rate reaches more than 95%, which is a very ideal method for efficiently separating and recovering components of waste polyester-cotton blended textiles.

[0108] It should be noted that, although the above embodiments have been described in this article, the patent protection scope of the present invention is not limited thereby. Therefore, based on the innovative concept of the present invention, changes and modifications made to the embodiments described herein, or equivalent structures or equivalent process changes made using the contents of the present invention specification and drawings, directly or indirectly applying the above technical solutions to other related technical fields, are all included in the patent protection scope of the present invention.

Claims

1. A method for separating components of waste polyester-cotton blended fabrics based on composite acid, characterized in that: The following steps are involved: The pre-treated waste polyester-cotton blended fabric is placed in a composite acid system, wherein the composite acid system includes an organic acid, an inorganic acid and a Lewis acid, and heated and degraded to obtain a reacted polyester-cotton mixture; The polyester-cotton mixture after the reaction is ultrasonically cleaned; Solid-liquid separation, recovery of polyester and cotton fibers respectively.

2. The method according to claim 1, characterized in that In the composite acid system, the mass concentration of the organic acid is 60-80wt%, the mass concentration of the inorganic acid is 1-5wt%, and the mass concentration of the Lewis acid is 1-5wt%.

3. The method according to claim 1, characterized in that: The organic acid is one of oxalic acid, p-toluenesulfonic acid, malic acid, acetic acid and citric acid; the inorganic acid is one of sulfuric acid, hydrochloric acid and phosphoric acid; and the Lewis acid is aluminum trichloride or zinc dichloride tetrahydrate.

4. The method according to claim 3, characterized in that The organic acid is oxalic acid.

5. The method according to claim 1, characterized in that The temperature of the heating degradation is 95-115° C. and the time is 1-3 hours.

6. The method according to claim 1, characterized in that The temperature of the ultrasonic cleaning is 50-70°C and the time is 10-30 minutes.

7. The method according to claim 1, characterized in that The cotton fiber content in the waste polyester-cotton blended fabric is 1-99wt%.

8. The method according to claim 1, characterized in that The solid-liquid separation comprises the following steps: The mixed solution after ultrasonic cleaning is initially filtered to obtain recovered polyester fibers and a preliminary filtrate; The preliminary filtrate is filtered and recovered again by vacuum suction drainage to obtain cotton fibers.

9. The method according to claim 1, characterized in that: The solid-liquid mass ratio of the pre-treated waste polyester-cotton blended fabric to the composite acid system is 1:10-100.

10. The method according to claim 1, characterized in that The following steps are also included: The filtrate after the solid-liquid separation is recovered to obtain a mixed solution containing organic acid crystals, and the mixed solution is placed in an environment of 2-4°C and cooled for 16-24 hours to obtain fully crystallized organic acid, which is further filtered to obtain wet organic acid crystals, which are placed in a vacuum environment and heated to obtain dry, high-purity organic acid crystals.

Citation Information

Patent Citations

  • Method for preparing small molecular weight organic acids through hydrothermal liquefaction of seaweed

    CN105111068A

  • Process for polyester-cotton fabric separation and microcrystalline cellulose preparation

    CN108424466A

  • Universal method for increasing value of cellulose waste textiles

    CN116829323A

  • Acid catalysis controllable degradation and recovery method for waste polyester and cotton-polyester blended fabric

    CN117024264A

  • Method for separating and recycling a waste polyester-cotton textile by means of a hydrothermal reaction catalyzed by an organic acid

    US20200262108A1

Cited By

  • Method for separating waste cotton-polyester blended fabric through subcritical water catalytic acidolysis

    CN119798777A

  • Degradation method of polyester-cotton fabric

    CN121021286A