Low-temperature-resistant and wet-skid-resistant tire rubber composition and screening method thereof
By combining solution-polymerized styrene-butadiene rubber and cis-butadiene rubber with specific microstructures and using nuclear magnetic resonance imaging, the balance between low-temperature resistance and wet skid resistance of tire rubber compositions was solved, achieving an efficient screening method and reducing development costs and time.
Patent Information
- Application Number
- CN202411179440.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies cannot effectively balance the design of solution-polymerized styrene-butadiene rubber and butadiene rubber, resulting in a difficulty in balancing the low-temperature resistance and wet skid resistance of tire rubber compositions. Furthermore, traditional screening methods are labor-intensive and inefficient.
By designing a combination of solution-polymerized styrene-butadiene rubber with a specific microstructure and a specific content of cis-butadiene rubber, and combining the microstructure of solution-polymerized styrene-butadiene rubber with nuclear magnetic resonance imaging, parameters for low-temperature resistance and wet skid resistance were established, and tire rubber compositions that take into account both properties were screened out.
This technology enables tire rubber compositions to maintain both low-temperature resistance and wet skid resistance at temperatures as low as -50°C, shortening the development cycle and reducing workload and costs.
Smart Images

Figure BDA0005011667330000051 
Figure BDA0005011667330000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber compositions, and in particular relates to a low-temperature-resistant and anti-slip tire rubber composition and a screening method thereof. Background Art
[0002] The low temperature resistance and wet skid resistance of tires are closely related to their minimum operating temperature and driving safety, respectively. Generally speaking, the lower the styrene content and vinyl content on the molecular chain of solution-polymerized styrene-butadiene rubber, the lower its brittle temperature and the better the low temperature resistance of the rubber material. However, the lower styrene content and vinyl content on the molecular chain of solution-polymerized styrene-butadiene rubber lead to a low glass transition temperature, so that the loss factor (tanδ@0℃) of the rubber around 0℃ is small, and the wet skid resistance of the tire is poor. Therefore, it is difficult to take into account both low temperature resistance and wet skid resistance using solution-polymerized styrene-butadiene rubber alone.
[0003] At present, in order to obtain a tire tread rubber composition that is resistant to low temperature and wet skid, a solution-polymerized styrene-butadiene rubber and cis-1,4-dimethylbutyl rubber are usually used for the design. However, since there are hundreds of brands of solution-polymerized styrene-butadiene rubber, how to select a suitable solution-polymerized styrene-butadiene rubber and cis-1,4-dimethylbutyl rubber for the design to obtain a tire rubber composition that takes into account both low temperature resistance and wet skid resistance is still a difficult problem in the current industry. Moreover, the current development of a tire rubber composition that takes into account both low temperature resistance and wet skid resistance can only be achieved by mixing all the schemes one by one according to the formula scheme and testing and verifying them. The specific implementation method is as follows: select different rubbers and ratios for test verification, perform banbury mixing, open refining, and sample preparation on all the formula schemes, use a flat vulcanizer for vulcanization, and use a low-temperature brittleness tester and a dynamic thermomechanical analyzer to test the low temperature resistance and dynamic mechanical properties of all samples, respectively, and abandon the schemes whose low temperature resistance and wet skid resistance do not meet the target. If a suitable scheme is not selected, all schemes are abandoned for the next round of scheme design and verification until a suitable scheme is selected. This implementation method requires a lot of manpower, material resources and financial resources to realize, resulting in huge waste of labor, material and testing costs, and the workload is heavy, which seriously affects development efficiency.
[0004] Therefore, providing a low-temperature resistant and anti-skid tire rubber composition and a screening method thereof is of great significance to those skilled in the art. Summary of the invention
[0005] The present invention aims at the technical problem in the prior art of how to select suitable solution-polymerized styrene-butadiene rubber and cis-1,4-butadiene rubber to design a tire rubber composition with both low-temperature resistance and anti-skid performance, and proposes a low-temperature resistant and anti-skid tire rubber composition and a screening method thereof. The present invention obtains a tire tread rubber composition with both low-temperature resistance and anti-skid performance by designing a solution-polymerized styrene-butadiene rubber with a specific microscopic composition and a cis-1,4-butadiene rubber with a specific content, which is conducive to shortening the product development cycle, reducing workload and saving costs.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is: a low temperature resistant and anti-slip tire rubber composition, including solution-polymerized styrene-butadiene rubber and butadiene rubber, the low temperature resistance performance parameter a and the anti-slip performance parameter b satisfy the following relationship: a<0.6 and b>0.53, wherein,
[0007] a=1.5×W S ×St S +W S ×Vi S , b=(1.4×St S +0.85×Vi S )×(W S +0.67×W B ×
[0008] |2.72×St S -0.69×Vi S |),
[0009] Where W S St represents the mass percentage of solution-polymerized styrene-butadiene rubber in the raw rubber system. S Indicates the mass percentage of styrene groups in the molecular chain of solution-polymerized styrene-butadiene rubber, Vi S Indicates the mass percentage of vinyl in the molecular chain of solution-polymerized styrene-butadiene rubber; W B It indicates the mass percentage of butadiene rubber in the blended rubber system.
[0010] In some of the embodiments, the low-temperature resistant and wet-skid resistant tire rubber composition can withstand temperatures as low as -50°C.
[0011] In some of the embodiments, the mass percentage of butadiene rubber in the blended rubber system is 30% to 40%.
[0012] In some of the embodiments, the butadiene rubber is a high-cis butadiene rubber, wherein the cis 1,4 structure content of the butadiene rubber is greater than 96%.
[0013] In some of the embodiments, the mass percentage of styrene groups in the molecular chain of the solution-polymerized styrene-butadiene rubber is 21% to 45%.
[0014] In some of the embodiments, the raw material components of the low temperature resistant and anti-skid tire rubber composition also include 70-120 parts of filler, 20-50 parts of plasticizer, 3-5 parts of activator, 2-5 parts of antioxidant, 5-12 parts of silane coupling agent, 1-2 parts of vulcanizer, and 3-5 parts of accelerator, by weight.
[0015] The present invention also provides a method for screening the above-mentioned low temperature resistant and anti-slip tire rubber composition, comprising the following steps:
[0016] The microscopic composition of the solution polymerized styrene butadiene rubber was characterized by nuclear magnetic resonance, and the mass percentage of styrene groups in the molecular chain of the solution polymerized styrene butadiene rubber was obtained. S and the mass percentage of vinyl Vi S ;
[0017] Based on the mass percentage of styrene groups in the molecular chain of solution polymerized styrene butadiene rubber (St) S and the mass percentage of vinyl Vi S , and the mass percentage of solution polymerized styrene-butadiene rubber in the rubber system W S , mass percentage of butadiene rubber W B , respectively establish low temperature resistance performance parameter relationship formulas, and according to the numerical values of the low temperature resistance performance parameters and the anti-wet skid performance parameters, realize the screening of low temperature resistant and anti-wet skid resistant tire rubber compositions.
[0018] In some embodiments, the low temperature resistance performance parameter a=1.5×W S ×St S +W S ×Vi S .
[0019] In some embodiments, the anti-skid performance parameter relationship b = (1.4 × St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |).
[0020] In some of the embodiments, if a>0.6, the low temperature resistance of the tire rubber composition is poor;
[0021] If b < 0.53, the anti-skid performance of the tire rubber composition is poor;
[0022] If a<0.6 and b>0.53, the tire rubber composition can have both low temperature resistance and wet skid resistance.
[0023] Compared with the prior art, the advantages and positive effects of the present invention are as follows: the low-temperature resistant and anti-slippery tire rubber composition of the present invention can take into account both low-temperature resistance and anti-slippery performance; the screening method of the low-temperature resistant and anti-slippery tire rubber of the present invention is simple to operate, and by selecting a solution-polymerized styrene-butadiene rubber and butadiene rubber with a specific microscopic composition and content, the tire tread rubber composition takes into account both low-temperature resistance and anti-slippery performance, which is conducive to shortening the product development cycle, reducing workload, and saving costs. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The embodiment of the present invention provides a low temperature resistant and wet-slip resistant tire rubber composition and a screening method thereof, wherein a tire tread rubber composition having both low temperature resistance and wet-slip resistance is obtained by combining a solution-polymerized styrene-butadiene rubber with a specific microscopic composition and a specific content of cis-butadiene rubber. The screening method of the present invention is simple to operate, and is conducive to shortening the product development cycle, reducing workload, and saving costs.
[0026] The low temperature resistant and anti-slip tire rubber composition provided by the embodiment of the present invention is resistant to low temperatures of minus 50°C, and includes solution-polymerized styrene-butadiene rubber and butadiene rubber, wherein the low temperature resistance performance parameter a and the anti-slip performance parameter b satisfy the following relationship: a<0.6 and b>0.53, and the low temperature resistance performance parameter a of the low temperature resistant and anti-slip tire rubber composition is 1.5×W S ×St S +W S ×Vi S , where a represents the low temperature resistance performance parameter, W S St represents the mass percentage of solution-polymerized styrene-butadiene rubber in the raw rubber system. S Indicates the mass percentage of styrene groups in the molecular chain of solution-polymerized styrene-butadiene rubber, Vi S It represents the mass percentage of vinyl in the molecular chain of solution-polymerized styrene-butadiene rubber; and the anti-wet skid performance parameter b of the low-temperature resistant and anti-wet skid resistant tire rubber composition is (1.4×St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |), where b represents the anti-skid performance parameter, W B It indicates the mass percentage of cis-1,4-butadiene rubber in the blended rubber system. The low temperature resistance performance parameters and wet skid resistance performance parameters are established by characterizing the styrene content and vinyl content in the solution polymerized styrene butadiene rubber molecular chain, as well as the content of solution polymerized styrene butadiene rubber and cis-1,4-butadiene rubber in the blended rubber system.
[0027] In the low temperature resistant and anti-slip tire rubber composition provided by the embodiment of the present invention, the mass percentage of cis-1,4-butadiene rubber in the combined rubber raw rubber system is 30% to 40%. In a preferred embodiment, the cis-1,4-butadiene rubber is high cis-1,4-butadiene rubber, and its cis-1,4-structure content is above 96%. By limiting the amount and structure of cis-1,4-butadiene rubber, the present invention has a low glass transition temperature, good molecular chain flexibility, and excellent low temperature resistance.
[0028] In the low-temperature and anti-skid tire rubber composition provided by the embodiment of the present invention, the solution polymerized styrene butadiene rubber is a medium styrene-based solution polymerized styrene butadiene rubber or a high styrene-based solution polymerized styrene butadiene rubber, the mass percentage of styrene in the solution polymerized styrene butadiene rubber molecular chain is 21% to 45%, the glass transition temperature is high, and the anti-skid performance is good.
[0029] The raw material components of the low-temperature resistant and anti-skid tire rubber composition provided by the embodiment of the present invention, measured by weight, also include 70-120 parts of filler, 20-50 parts of plasticizer, 3-5 parts of activator, 2-5 parts of antioxidant, 5-12 parts of silane coupling agent, 1-2 parts of vulcanizer, and 3-5 parts of accelerator.
[0030] The method for screening a low temperature resistant and wet-slip resistant tire rubber composition provided in an embodiment of the present invention specifically comprises the following steps:
[0031] The styrene content and vinyl content in the solution polymerized styrene butadiene rubber molecular chain were characterized by nuclear magnetic resonance spectroscopy, and the mass percentage of styrene in the solution polymerized styrene butadiene rubber molecular chain was obtained. S The mass percentage of vinyl in the molecular chain of solution-polymerized styrene-butadiene rubber is Vi S ;
[0032] Based on the mass percentage of styrene groups in the molecular chain of solution polymerized styrene butadiene rubber (St) S and the mass percentage of vinyl Vi S , and the mass percentage of solution polymerized styrene-butadiene rubber in the rubber system W S , mass percentage of butadiene rubber W B , establish the low temperature resistance related parameters a = 1.5 × W S ×St S +W S ×Vi S And the anti-skid performance related parameters b = (1.4 × St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |), according to the numerical values of the low temperature resistance performance parameter and the anti-skid performance parameter, the screening of the low temperature resistance and anti-skid tire rubber composition is achieved.
[0033] If the low temperature resistance performance parameter a>0.6, the low temperature resistance performance of the tire rubber composition is poor;
[0034] If the anti-skid performance parameter b is less than 0.53, the anti-skid performance of the tire rubber composition is poor;
[0035] If a<0.6 and b>0.53, the tire rubber composition can have both low temperature resistance and wet skid resistance.
[0036] In order to more clearly and in detail introduce the low-temperature resistant and anti-skid tire rubber composition and the screening method thereof provided by the embodiments of the present invention, they will be described below in conjunction with specific embodiments.
[0037] The formulations of the tire rubber compositions of the embodiments of the present invention and the comparative examples are shown in Table 1.
[0038] Table 1. Formula and microstructure of tire rubber compositions of Examples 1-7 and Comparative Examples 1-5
[0039]
[0040] Note: The number of raw rubber parts is calculated based on dry rubber
[0041] Example 1
[0042] Raw material formula: 30 parts of cis-1,4-dibutyl rubber; 70 parts of solution-polymerized styrene-butadiene rubber, wherein the mass percentage of styrene groups in the molecular chain of the solution-polymerized styrene-butadiene rubber is 21% and the mass percentage of vinyl groups is 50%;
[0043] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; activator is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts.
[0044] The tire rubber composition of this embodiment is mixed and vulcanized according to the following steps:
[0045] S1. Add cis-butadiene rubber, solution-polymerized styrene-butadiene rubber, zinc oxide, stearic acid, 6PPD, wax, SiO 2 and solid silane coupling agent Si69, press and mix for 40 seconds or to 115°C, with the internal mixer rotating at 90 rpm;
[0046] S2, lift the plug to clean, press the plug to mix for 40 seconds or to 135℃, the speed of the internal mixer is 90rpm;
[0047] S3, after lifting the bolt, press the bolt and mix for 30 seconds or to 145°C, with the internal mixer rotating at 90 rpm;
[0048] S4, lift the plug and then press the plug, mix at a constant temperature of 145°C for 180s, discharge the rubber and cool the sheet to obtain a masterbatch;
[0049] S5, lift the plug and add the masterbatch, sulfur, accelerator CZ, accelerator DPG, press the plug and mix for 30 seconds or to 85°C, the internal mixer speed is 60rpm;
[0050] S6, after lifting the bolt, press the bolt and mix to 100°C, with the internal mixer rotating at 60 rpm;
[0051] S7, after lifting the plug, press the plug and mix for 30 seconds or until the temperature reaches 110°C, discharge the rubber and cool the sheet to obtain the final rubber mix;
[0052] S8. Vulcanize the final rubber mixture on a flat vulcanizer at 161° C. under a pressure of 12 MPa for 20 min to obtain a tire rubber composition.
[0053] Example 2
[0054] Compared with Example 1, the content of styrene and vinyl in the solution polymerized styrene butadiene rubber molecular chain in the tire rubber composition raw material of this embodiment is different. The raw material formula of this embodiment is: 30 parts of cis-butadiene rubber; 70 parts of solution polymerized styrene butadiene rubber, and the mass percentage of styrene in the solution polymerized styrene butadiene rubber molecular chain is 28%, and the mass percentage of vinyl is 42%;
[0055] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; activator is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts.
[0056] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.
[0057] Example 3
[0058] Compared with Example 1, the content of styrene and vinyl in the molecular chain of the solution polymerized styrene butadiene rubber in the raw materials of the tire rubber composition of this embodiment is different. The raw material formula of this embodiment is: 30 parts of cis-butadiene rubber; 70 parts of solution polymerized styrene butadiene rubber, and the mass percentage of styrene in the molecular chain of the solution polymerized styrene butadiene rubber is 36%, and the mass percentage of vinyl is 26%;
[0059] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; activator is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts.
[0060] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.
[0061] Example 4
[0062] Compared with Example 1, the content of styrene and vinyl in the solution polymerized styrene butadiene rubber molecular chain in the tire rubber composition raw material of this embodiment is different. The raw material formula of this embodiment is: 30 parts of cis-butadiene rubber; 70 parts of solution polymerized styrene butadiene rubber, and the mass percentage of styrene in the solution polymerized styrene butadiene rubber molecular chain is 40%, and the mass percentage of vinyl is 14%;
[0063] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; activator is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts.
[0064] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.
[0065] Example 5
[0066] Compared with Example 2, the amounts of solution polymerized styrene-butadiene rubber and cis-butadiene rubber in the raw material and raw rubber system of the tire rubber composition of this embodiment are different. The raw material formula of this embodiment is: 40 parts of cis-butadiene rubber; 60 parts of solution polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the molecular chain of the solution polymerized styrene-butadiene rubber is 28%, and the mass percentage of vinyl groups is 42%;
[0067] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; active agent is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts;
[0068] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.
[0069] Example 6
[0070] Compared with Example 3, the amounts of solution polymerized styrene-butadiene rubber and cis-butadiene rubber in the raw material and rubber system of the tire rubber composition of this embodiment are different. The raw material formula of this embodiment is: 40 parts of cis-butadiene rubber; 60 parts of solution polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the molecular chain of the solution polymerized styrene-butadiene rubber is 36%, and the mass percentage of vinyl groups is 26%;
[0071] Filler is SiO 280 parts; plasticizer is 37.5 parts; active agent is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts;
[0072] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.
[0073] Example 7
[0074] Compared with Example 4, the amounts of solution polymerized styrene-butadiene rubber and cis-butadiene rubber in the raw material and raw rubber system of the tire rubber composition of this embodiment are different. The raw material formula of this embodiment is: 40 parts of cis-butadiene rubber; 60 parts of solution polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the molecular chain of the solution polymerized styrene-butadiene rubber is 40%, and the mass percentage of vinyl groups is 14%;
[0075] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; active agent is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts;
[0076] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.
[0077] Comparative Example 1
[0078] Compared with Example 1, the vinyl content in the solution polymerized styrene butadiene rubber molecular chain in the tire rubber composition raw materials of this comparative example is different. The raw material formula of this comparative example is: 30 parts of cis-butadiene rubber; 70 parts of solution polymerized styrene butadiene rubber, and the mass percentage of styrene groups in the solution polymerized styrene butadiene rubber molecular chain is 21%, and the mass percentage of vinyl groups is 43%;
[0079] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; active agent is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts;
[0080] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those of Example 1.
[0081] Comparative Example 2
[0082] Compared with Example 4, the raw rubber system of the tire rubber composition of this comparative example is solution polymerized styrene butadiene rubber. The raw material formula of this comparative example is: 100 parts of solution polymerized styrene butadiene rubber, and the mass percentage of styrene groups in the molecular chain of the solution polymerized styrene butadiene rubber is 40%, and the mass percentage of vinyl groups is 14%;
[0083] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; activator is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts.
[0084] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those of Example 1.
[0085] Comparative Example 3
[0086] Compared with Example 3, the amount of solution polymerized styrene-butadiene rubber and cis-butadiene rubber in the raw material and raw rubber system of the tire rubber composition of this comparative example is different. The raw material formula of this comparative example is: 10 parts of cis-butadiene rubber; 90 parts of solution polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the molecular chain of the solution polymerized styrene-butadiene rubber is 36%, and the mass percentage of vinyl groups is 26%;
[0087] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; active agent is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts;
[0088] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those of Example 1.
[0089] Comparative Example 4
[0090] Compared with Example 5, the content of styrene and vinyl in the molecular chain of the solution polymerized styrene-butadiene rubber of the tire rubber composition of this comparative example is different. The raw material formula of this comparative example is: 40 parts of cis-butadiene rubber; 60 parts of solution polymerized styrene-butadiene rubber, and the mass percentage of styrene in the molecular chain of the solution polymerized styrene-butadiene rubber is 21%, and the mass percentage of vinyl is 43%;
[0091] Filler is SiO 2 80 parts; plasticizer is 37.5 parts; active agent is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts;
[0092] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those of Example 1.
[0093] Comparative Example 5
[0094] Compared with Example 1, the raw rubber system of the tire rubber composition of this comparative example is butadiene rubber, and the raw material formula of this comparative example is: 100 parts of butadiene rubber; the filler is SiO 2 80 parts; plasticizer is 37.5 parts; activator is zinc oxide 3 parts, stearic acid 2 parts; antioxidant is antioxidant 6PPD 2 parts, wax 1 part; silane coupling agent is solid Si69 12.8 parts; vulcanizing agent is sulfur 1.5 parts; accelerator CZ 2 parts, accelerator DPG 2 parts.
[0095] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those of Example 1.
[0096] Performance Testing
[0097] The tire rubber compositions prepared in Examples 1-7 and Comparative Examples 1-5 were tested for low temperature resistance and anti-skid performance, and the test results were recorded. The test results were compared with the low temperature resistance related parameter a and anti-skid performance related parameter b of the tire rubber compositions prepared in Examples 1-7 and Comparative Examples 1-5 calculated according to the screening method of the present invention, and the results are shown in Table 2.
[0098] Among them, the low temperature resistance is measured using a low temperature brittleness tester (Japan Ueshima Co., Ltd., model TM-2135) according to the national standard GB / T 15256-2014 "Determination of low temperature brittleness of vulcanized rubber or thermoplastic rubber (multiple specimen method)" to measure the brittle temperature of each tire tread rubber composition. The lower the brittle temperature, the better the low temperature resistance;
[0099] The anti-skid performance was measured using a dynamic thermal mechanical analyzer DMA (NETZSCH, Germany, model EPLEXOR 500N) at a frequency of 10 Hz, a static strain of 7% and a dynamic strain of 0.25%. The loss factor (tanδ) of each tire tread rubber composition at different temperatures was measured. The larger the loss factor of tanδ@0°C, the better the anti-skid performance. The results were expressed as an index, and the result of Comparative Example 1 was set to 100. The larger the index, the better the anti-skid performance.
[0100] Table 2 Performance of tire rubber compositions of Examples 1-7 and Comparative Examples 1-5
[0101]
[0102] As can be seen from the above, Comparative Example 2 corresponds to Example 4, and Comparative Example 3 corresponds to Example 3. Compared with the examples, the rubber compositions obtained in Comparative Examples 2 and 3 have good anti-skid performance, but poor low temperature resistance; Comparative Example 4 corresponds to Example 5, and Comparative Example 5 corresponds to Example 1. Compared with the examples, the rubber compositions of Comparative Examples 4 and 5 have good low temperature resistance, but poor anti-skid performance.
[0103] Moreover, according to the screening method for low-temperature-resistant and wet-skid-resistant tire rubber compositions provided by the present invention, the low-temperature resistance performance-related parameter a of the tire rubber compositions prepared in Examples 1-7 is <0.6, and the wet-skid-resistant performance-related parameter b is >0.53, indicating that the tire rubber compositions of the embodiments of the present invention can take into account both low-temperature resistance and wet-skid resistance; after performance testing, the brittle temperatures of the tire rubber compositions prepared in Examples 1-7 are all below -50°C, and the loss factors of tanδ@0°C are all greater than those of Comparative Example 1, which is consistent with the judgment results of the screening method for low-temperature-resistant and wet-skid-resistant tire rubber compositions provided by the present invention, indicating that the tire rubber compositions obtained by the screening method for low-temperature-resistant and wet-skid-resistant tire rubber compositions of the present invention can take into account both low-temperature resistance and wet-skid resistance of the tire rubber compositions.
[0104] The above-described embodiments are merely descriptions of preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various deformations, modifications, evolutions, and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the scope of protection determined by the claims of the present invention.
Claims
1. A low temperature resistant and anti-skid tire rubber composition, characterized in that: Including solution-polymerized styrene-butadiene rubber and butadiene rubber, the low temperature resistance performance parameter a and the anti-slip performance parameter b satisfy the following relationship: a<0.6 and b>0.53, wherein, a=1.5×W S ×St S +W S ×Vi S ,b=(1.4×St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |), Where W S St represents the mass percentage of solution-polymerized styrene-butadiene rubber in the raw rubber system. S Indicates the mass percentage of styrene groups in the molecular chain of solution-polymerized styrene-butadiene rubber, Vi S Indicates the mass percentage of vinyl in the molecular chain of solution-polymerized styrene-butadiene rubber; W B It indicates the mass percentage of butadiene rubber in the blended rubber system.
2. The low temperature resistant and wet skid resistant tire rubber composition according to claim 1, characterized in that: The low-temperature-resistant and anti-slip tire rubber composition can withstand temperatures as low as -50°C.
3. The low temperature resistant and wet skid resistant tire rubber composition according to claim 1, characterized in that: The mass percentage of butadiene rubber in the blended rubber system is 30% to 40%.
4. The low temperature resistant and wet skid resistant tire rubber composition according to claim 1, characterized in that: Butyl rubber is a high cis-butadiene rubber, and its cis-1,4 structure content is above 96%.
5. The low temperature resistant and wet skid resistant tire rubber composition according to claim 1, characterized in that: The mass percentage of styrene groups in the solution polymerized styrene-butadiene rubber molecular chain is 21% to 45%.
6. The low temperature resistant and wet skid resistant tire rubber composition according to claim 1, characterized in that: Calculated by weight, the raw material components of the low-temperature resistant and anti-skid tire rubber composition also include 70-120 parts of filler, 20-50 parts of plasticizer, 3-5 parts of activator, 2-5 parts of antioxidant, 5-12 parts of silane coupling agent, 1-2 parts of vulcanizer, and 3-5 parts of accelerator.
7. The method for screening a low temperature resistant and wet skid resistant tire rubber composition according to any one of claims 1 to 6, characterized in that: The following steps are involved: The microscopic composition of the solution polymerized styrene butadiene rubber was characterized by nuclear magnetic resonance, and the mass percentage of styrene groups in the molecular chain of the solution polymerized styrene butadiene rubber was obtained. S and the mass percentage of vinyl Vi S ; Based on the mass percentage of styrene groups in the molecular chain of solution polymerized styrene butadiene rubber (St) S and the mass percentage of vinyl Vi S , and the mass percentage of solution polymerized styrene-butadiene rubber in the rubber system W S , mass percentage of butadiene rubber W B , respectively establish low temperature resistance performance parameter relationship formulas, and according to the numerical values of the low temperature resistance performance parameters and the anti-wet skid performance parameters, realize the screening of low temperature resistant and anti-wet skid resistant tire rubber compositions.
8. The method for screening a low-temperature resistant and wet-skid resistant tire rubber composition according to claim 7, characterized in that: Low temperature resistance performance parameter a=1.5×W S ×St S +W S ×Vi S .
9. The method for screening a low temperature resistant and wet skid resistant tire rubber composition according to claim 8, characterized in that: Anti-skid performance parameter relationship b = (1.4 × St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |).
10. The method for screening a low temperature resistant and wet skid resistant tire rubber composition according to claim 9, characterized in that: If a>0.6, the low temperature resistance of the tire rubber composition is poor; If b < 0.53, the anti-skid performance of the tire rubber composition is poor; If a<0.6 and b>0.53, the tire rubber composition can have both low temperature resistance and wet skid resistance.