High-temperature-resistant plastic particles and preparation method thereof
By introducing high-temperature resistance additives containing ether bonds and triazine rings and modified antioxidants with glycidyl ester groups into high-density polyethylene, the problem of insufficient heat resistance of high-density polyethylene in high-temperature environments is solved, and the heat resistance performance of high-density polyethylene is significantly improved. The high temperature and oxidation resistance of plastic particles.
Patent Information
- Application Number
- CN202410868619.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing high-density polyethylene has insufficient heat resistance in high-temperature environments, and the poor solubility of triaryl-matriazine polymers limits its application in the plastic field.
Using a high-temperature resistant plastic particles, including high-density polyethylene, high-temperature resistant additives and modified antioxidants, the high-temperature resistant additives containing ether bonds and triazine rings are synthesized through specific process steps, and in alkaline The modified antioxidant formed with glycidyl ester groups under conditions improves the high temperature and antioxidant properties of the polymer.
It improves the high-temperature resistance and oxidation resistance of plastic particles, enhances the thermal decomposition temperature and processing properties of polymers, and ensures stability and chemical corrosion resistance in high-temperature environments.
Smart Images

Figure BDA0004920965940000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to high temperature resistant plastic particles and a preparation method thereof. Background Art
[0002] High-density polyethylene is a highly crystalline, non-polar thermoplastic polymer. It has high strength, good chemical corrosion resistance, excellent electrical insulation and processing convenience. It is widely used in aerospace, electronic devices, automobile manufacturing and other industries. However, with the continuous improvement of technology and market demand, the heat resistance of high-density polyethylene needs to be continuously modified to extend the life of high-density polyethylene in more harsh high-temperature environments.
[0003] In the prior art, triaryl-s-triazine, as a nitrogen-containing heterocyclic compound, has excellent thermal stability and high temperature resistance due to the conjugation effect of the aromatic ring and the nitrogen atom in its molecular structure. Therefore, introducing aromatic-s-triazine into a polymer can enhance the high temperature resistance and chemical corrosion resistance of the polymer. However, linear triaryl-s-triazine polymers generally have poor solubility and are difficult to process, which limits the application of triaryl-s-triazine polymers in plastics. Summary of the invention
[0004] The object of the present invention is to provide a high temperature resistant plastic particle and a preparation method thereof, so as to solve the problems in the background technology.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A high temperature resistant plastic granule, comprising the following raw materials in parts by weight:
[0007] 110-120 parts of high-density polyethylene, 8-13 parts of high-temperature resistant additives, 0.5-1 parts of plasticizers, 0.3-0.5 parts of defoamers, 4-8 parts of modified antioxidants;
[0008] The high temperature resistant auxiliary agent is prepared by the following steps:
[0009] A1. Add 4,4'-dihydroxydiphenyl sulfide and 4-nitrophthalonitrile to N,N-dimethylformamide, stir and mix, then add anhydrous potassium carbonate, stir and react at 80-90°C for 7-8h, cool, place in a 10wt% dilute hydrochloric acid solution, let stand for 6-8h, filter, wash with distilled water, and dry to obtain a benzonitrile monomer; use anhydrous potassium carbonate as an alkaline catalyst to react the hydroxyl group in 4,4'-dihydroxydiphenyl sulfide with the cyano group in 4-nitrophthalonitrile to obtain a benzonitrile monomer containing a sulfide bond;
[0010] A2. After the benzonitrile monomer is melted at 114-120° C., 4,4'-diaminodiphenyl sulfone is added, and the mixture is stirred for reaction for 10-30 minutes. The mixture is quenched, crushed, and vacuumed, and then placed in a muffle furnace for high-temperature treatment. After cooling, a high-temperature resistant additive is obtained. 4,4'-diaminodiphenyl sulfone is used as a curing agent and catalyst to initiate a polymerization reaction with the benzonitrile monomer to generate a cross-linked structure containing a triazine ring and an isoindoline group in the main chain.
[0011] Furthermore, the high temperature treatment is performed by heating at a program of 250°C / 4h, 300°C / 4h, and 350°C / 4h.
[0012] Furthermore, the dosage ratio of the N,N-dimethylformamide, 4,4'-dihydroxydiphenyl sulfide, 4-nitrophthalonitrile, anhydrous potassium carbonate and hydrochloric acid solution is 50mL: 4-5g: 8-9g: 6-9g: 300mL.
[0013] Furthermore, the usage ratio of the benzonitrile monomer and 4,4'-diaminodiphenyl sulfone is 9-10g:0.5g.
[0014] Furthermore, the modified antioxidant is prepared by the following steps:
[0015] Gallic acid is added to anhydrous ethanol, and after stirring and mixing at 60° C., a potassium hydroxide / anhydrous ethanol mixture is added to adjust the pH value to 9-10, and then epichlorohydrin is added dropwise in a nitrogen atmosphere, and the mixture is stirred and reacted at 70-80° C. for 6-8 hours. After cooling, glacial acetic acid is added to adjust the pH value to 6.5-7, and the mixture is filtered, washed with anhydrous ethanol and deionized water, and dried to obtain a modified antioxidant; under alkaline conditions, the epoxy group of epichlorohydrin is ring-opened to form an active center, and the phenolic hydroxyl group of gallic acid can undergo a nucleophilic addition reaction with the ring-opened active center to form an ester bond, and then an intramolecular ring closure occurs to generate gallic acid containing a glycidyl ester group.
[0016] Furthermore, the dosage ratio of anhydrous ethanol, gallic acid and epichlorohydrin is 50mL:8-12g:6-18mL; the potassium hydroxide / anhydrous ethanol mixed solution is composed of potassium hydroxide and anhydrous ethanol mixed in a dosage ratio of 0.5-2g:20mL.
[0017] A method for preparing high temperature resistant plastic particles comprises the following steps:
[0018] High-density polyethylene, high-temperature resistant additives, plasticizers, defoamers, and modified antioxidants are added to a high-speed mixer for stirring and mixing, and then added to a screw extruder for extrusion, and then cooled and pelletized to obtain high-temperature resistant plastic particles.
[0019] Beneficial effects of the present invention:
[0020] The high temperature resistant additive of the present invention contains an ether bond with good flexibility. When blended with high-density polyethylene, it helps to improve the movement of the high temperature resistant additive in the high-density polyethylene molecular chain, and enhances the interaction between the high temperature resistant additive and the high-density polyethylene through van der Waals force, thereby improving the processing performance of the high temperature resistant additive in the high-density polyethylene matrix, so that the high temperature resistant additive is evenly dispersed in the high-density polyethylene matrix and forms a complex molecular chain entanglement. At the same time, there is a strong charge transfer interaction between the triazine ring and the isoindoline group introduced in the high temperature resistant additive, which increases the thermal decomposition temperature of the high-density polyethylene when heated, thereby enhancing the high temperature resistance of the prepared plastic particles;
[0021] The modified antioxidant of the present invention contains a hydrophobic glycidyl ester group, and when blended with high-density polyethylene, it can be combined with the high-density polyethylene through the Van der Waals force to enhance the intermolecular force, thereby improving the interfacial compatibility between the modified antioxidant and the high-density polyethylene. At the same time, the modified antioxidant contains abundant phenolic hydroxyl groups, which can effectively capture free radicals triggered by heat, light or oxygen, interrupt the chain thermal oxidation reaction, and improve the antioxidant performance of the obtained plastic particles.
[0022] The present invention uses high-density polyethylene as a base material, and improves the high-temperature resistance of the prepared plastic particles by introducing a high-temperature resistant auxiliary agent with good processability with the high-density polyethylene resin. At the same time, the introduction of the modified antioxidant effectively improves the oxidation resistance of the plastic particles. In addition, since the triazine ring and the isoindoline group in the high-temperature resistant auxiliary agent have good electron cloud distribution, additional free radical capture points can be provided for the modified antioxidant, further improving the oxidation resistance of the prepared plastic particles. At the same time, the modified antioxidant also has good thermal stability, which can further increase the thermal decomposition temperature of the prepared plastic particles. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1
[0025] This embodiment provides a high temperature resistant additive, which is prepared by the following steps:
[0026] A1. Add 4 g of 4,4'-dihydroxydiphenyl sulfide and 8 g of 4-nitrophthalonitrile to 50 mL of N,N-dimethylformamide, stir and mix, then add 6 g of anhydrous potassium carbonate, stir and react at 80°C for 7 h, cool, place in 300 mL of 10 wt% dilute hydrochloric acid solution, let stand for 6 h, filter, wash with distilled water, and dry to obtain a benzonitrile monomer;
[0027] A2. After 9 g of benzonitrile monomer was melted at 114° C., 0.5 g of 4,4'-diaminodiphenyl sulfone was added, and the mixture was stirred for 10 min. After quenching, powdering, and vacuuming, the mixture was placed in a muffle furnace and subjected to high temperature treatment at a temperature of 250° C. / 4 h. After cooling, a high temperature resistant additive was obtained.
[0028] Example 2
[0029] This embodiment provides a high temperature resistant additive, which is prepared by the following steps:
[0030] A1. Add 4.5 g of 4,4'-dihydroxydiphenyl sulfide and 8.5 g of 4-nitrophthalonitrile to 50 mL of N,N-dimethylformamide, stir and mix, then add 7 g of anhydrous potassium carbonate, stir and react at 85°C for 7.5 h, cool, place in 300 mL of 10 wt% dilute hydrochloric acid solution, let stand for 7 h, filter, wash with distilled water, and dry to obtain a benzonitrile monomer;
[0031] A2. After 9.5 g of benzonitrile monomer was melted at 118° C., 0.5 g of 4,4'-diaminodiphenyl sulfone was added, and the mixture was stirred for reaction for 20 min. The mixture was quenched, powdered, and vacuumed, and then placed in a muffle furnace for high-temperature treatment at a temperature of 300° C. / 4 h. After cooling, a high-temperature resistant additive was obtained.
[0032] Example 3
[0033] This embodiment provides a high temperature resistant additive, which is prepared by the following steps:
[0034] A1. Add 5 g of 4,4'-dihydroxydiphenyl sulfide and 9 g of 4-nitrophthalonitrile to 50 mL of N,N-dimethylformamide, stir and mix, then add 9 g of anhydrous potassium carbonate, stir and react at 90°C for 8 h, cool, place in 300 mL of 10 wt% dilute hydrochloric acid solution, let stand for 8 h, then filter, wash with distilled water, and dry to obtain a benzonitrile monomer;
[0035] A2. After 10 g of benzonitrile monomer was melted at 120° C., 0.5 g of 4,4'-diaminodiphenyl sulfone was added, and the mixture was stirred for reaction for 30 min. The mixture was quenched, powdered, and vacuumed, and then placed in a muffle furnace for high temperature treatment at a temperature of 350° C. / 4 h. After cooling, a high temperature resistant additive was obtained.
[0036] Example 4
[0037] This embodiment provides a modified antioxidant, which is prepared by the following steps:
[0038] Add 8 g of gallic acid to 50 mL of anhydrous ethanol, stir and mix at 60 ° C, add a mixture of potassium hydroxide and anhydrous ethanol in a dosage ratio of 0.5 g: 20 mL, adjust the pH value to 9, and then drop 6 mL of epichlorohydrin in a nitrogen atmosphere, stir and react at 70 ° C for 6 hours, cool, add glacial acetic acid to adjust the pH value to 6.5, and then filter, wash with anhydrous ethanol and deionized water, and dry to obtain a modified antioxidant.
[0039] Example 5
[0040] This embodiment provides a modified antioxidant, which is prepared by the following steps:
[0041] Add 10 g of gallic acid to 50 mL of anhydrous ethanol, stir and mix at 60 ° C, add a mixture of potassium hydroxide and anhydrous ethanol in a dosage ratio of 1 g: 20 mL, adjust the pH value to 9.5, and then drop 16 mL of epichlorohydrin in a nitrogen atmosphere, stir and react at 75 ° C for 7 hours, cool, add glacial acetic acid to adjust the pH value to 6.5, and then filter, wash with anhydrous ethanol and deionized water, and dry to obtain a modified antioxidant.
[0042] Example 6
[0043] This embodiment provides a modified antioxidant, which is prepared by the following steps:
[0044] 12 g of gallic acid was added to 50 mL of anhydrous ethanol, and the mixture was stirred at 60° C., and a mixture of potassium hydroxide and anhydrous ethanol in a ratio of 2 g: 20 mL was added, and the pH value was adjusted to 10. Then, 18 mL of epichlorohydrin was added dropwise in a nitrogen atmosphere, and the reaction was stirred at 80° C. for 8 hours. After cooling, glacial acetic acid was added to adjust the pH value to 7, and then the modified antioxidant was obtained after filtration, washing with anhydrous ethanol and deionized water, and drying.
[0045] Example 7
[0046] This embodiment provides a high temperature resistant plastic particle, comprising the following steps:
[0047] 110 parts by weight of high-density polyethylene, 8 parts by weight of high-temperature resistant additive, 0.5 parts by weight of plasticizer, 0.3 parts by weight of defoamer and 4 parts by weight of modified antioxidant are added into a high-speed mixer and stirred and mixed, then added into a screw extruder for extrusion, and then cooled and pelletized to obtain high-temperature resistant plastic particles.
[0048] Example 8
[0049] This embodiment provides a high temperature resistant plastic particle, comprising the following steps:
[0050] 115 parts by weight of high-density polyethylene, 10 parts by weight of high-temperature resistant additive, 0.5 parts by weight of plasticizer, 0.4 parts by weight of defoamer and 6 parts by weight of modified antioxidant are added into a high-speed mixer and stirred and mixed, then added into a screw extruder for extrusion, and then cooled and pelletized to obtain high-temperature resistant plastic particles.
[0051] Example 9
[0052] This embodiment provides a high temperature resistant plastic particle, comprising the following steps:
[0053] 120 parts by weight of high-density polyethylene, 13 parts by weight of high-temperature resistant additives, 1 part by weight of plasticizer, 0.5 parts by weight of defoaming agent, and 8 parts by weight of modified antioxidant are added into a high-speed mixer and stirred and mixed, then added into a screw extruder for extrusion, and then cooled and pelletized to obtain high-temperature resistant plastic particles.
[0054] Comparative Example 1: Compared with Comparative Example 7, an equal amount of the high temperature resistant additive is replaced with alumina, and the rest is the same.
[0055] Comparative Example 2: Compared with Comparative Example 7, no high temperature resistant additive is added, and the rest is the same.
[0056] Comparative Example 3: Compared with Example 7, the modified antioxidant was replaced with an equal amount of a commercially available antioxidant, and the rest was the same.
[0057] Performance tests were performed on Examples 7 to 9 and Comparative Examples 1 to 3. High temperature resistance test: the sample was placed in a thermogravimetric analyzer, and the temperature was raised from 20°C to 500°C at a heating rate of 10°C / min in a nitrogen atmosphere to test the initial decomposition temperature of the sample. Antioxidation test: the sample was placed in a thermal oxygen aging tester for thermal oxygen aging, and the thermal oxygen aging temperature was set to 100°C for 30 days. The elongation at break and tensile strength before and after oxidation were recorded. The tensile strength and elongation at break were based on the national standard GB / T 1040.1-2006. The results are shown in Table 1:
[0058] Table 1
[0059]
[0060] It can be seen from Table 1 that the plastic particles prepared from the high temperature resistant additives and the modified antioxidants in Examples 7-9 have an initial decomposition temperature significantly higher than that of the plastic particles prepared from Comparative Examples 1-3, and have good high temperature resistance; at the same time, the elongation at break and the impact strength before and after oxidation are higher than those of the plastic particles prepared from Comparative Examples 1-3; compared with Comparative Examples 1 and 3, Example 7 has a higher initial decomposition temperature, indicating that under the coordinated action of the high temperature resistant additives and the modified antioxidants, the obtained plastic particles have higher high temperature resistance and antioxidant properties.
[0061] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0062] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high temperature resistant plastic particle, characterized in that: It includes the following raw materials in parts by weight: 110-120 parts of high-density polyethylene, 8-13 parts of high-temperature resistant additives, 0.5-1 parts of plasticizers, 0.3-0.5 parts of defoamers, 4-8 parts of modified antioxidants; The high temperature resistant auxiliary agent is prepared by the following steps: A1. Add 4,4'-dihydroxydiphenyl sulfide and 4-nitrophthalonitrile to N,N-dimethylformamide, stir and mix, then add anhydrous potassium carbonate, stir and react at 80-90°C for 7-8h, cool, place in a 10wt% dilute hydrochloric acid solution, let stand for 6-8h, filter, wash with distilled water, and dry to obtain a benzonitrile monomer; A2. After the benzonitrile monomer is melted at 114-120° C., 4,4'-diaminodiphenyl sulfone is added, and the mixture is stirred for 10-30 minutes. The mixture is then quenched, crushed, and vacuumed, and then placed in a muffle furnace for high-temperature treatment. After cooling, a high-temperature resistant additive is obtained.
2. A high temperature resistant plastic particle according to claim 1, characterized in that: The dosage ratio of the N,N-dimethylformamide, 4,4'-dihydroxydiphenyl sulfide, 4-nitrophthalonitrile, anhydrous potassium carbonate and hydrochloric acid solution is 50mL: 4-5g: 8-9g: 6-9g: 300mL.
3. The high temperature resistant plastic particles according to claim 1, characterized in that: The usage ratio of the benzonitrile monomer and 4,4'-diaminodiphenyl sulfone is 9-10g:0.5g.
4. The high temperature resistant plastic particles according to claim 1, characterized in that: The high temperature treatment is performed by heating at a rate of 250°C / 4h, 300°C / 4h, and 350°C / 4h.
5. The high temperature resistant plastic particles according to claim 1, characterized in that: The modified antioxidant is prepared by the following steps: Gallic acid is added to anhydrous ethanol, and after stirring and mixing at 60° C., a potassium hydroxide / anhydrous ethanol mixture is added to adjust the pH value to 9-10, and then epichlorohydrin is added dropwise in a nitrogen atmosphere, and the reaction is stirred at 70-80° C. for 6-8 hours. After cooling, glacial acetic acid is added to adjust the pH value to 6.5-7, and then filtered, washed with anhydrous ethanol and deionized water, and dried to obtain a modified antioxidant.
6. The high temperature resistant plastic particles according to claim 5, characterized in that: The dosage ratio of the anhydrous ethanol, gallic acid and epichlorohydrin is 50mL:8-12g:6-18mL; the potassium hydroxide / anhydrous ethanol mixed solution is composed of potassium hydroxide and anhydrous ethanol mixed in a dosage ratio of 0.5-2g:20mL.
7. The method for preparing high temperature resistant plastic particles according to claim 1, characterized in that: The following steps are involved: High-density polyethylene, high-temperature resistant additives, plasticizers, defoamers, and modified antioxidants are added to a high-speed mixer for stirring and mixing, and then added to a screw extruder for extrusion, and then cooled and pelletized to obtain high-temperature resistant plastic particles.