High-flame-retardant polypropylene composite material and preparation method thereof

By blending benzylchloroyl chitosan, modified carbon nanotubes and silicon modified boric acid with polypropylene, high flame retardant polypropylene composite materials, the problems of insufficient antibacterial performance and flammable bacterial erosion in the prior art are solved. A significant flame retardant and antibacterial effects were achieved.

CN118931034AInactive Publication Date: 2024-11-12青岛海铁复合材料有限公司
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411006074.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing high thermal flame-retardant polypropylene composite materials have shortcomings in antibacterial properties, and the problems of flammability and bacterial erosion have not been effectively solved.

Method used

3-5 parts by weight of benzylchlorochitosan, 4-6 parts by weight of modified carbon nanotubes and 5-8 parts by weight of silicon modified boric acid and 60-80 parts by weight of polypropylene, through double The screw extrusion mechanism is equipped with a high flame retardant polypropylene composite material to generate quaternary ammonium groups with antibacterial effects, and the flame retardant effect is achieved through the combination of boric acid, sulfur elements and carbon nanotubes.

Benefits of technology

It significantly improves the flame retardant and antibacterial properties of the material. Boric acid forms a glass coating when burning, and sulfuric acid and carbon layers play a role in insulating and insulating the carbon nanotube itself has a flame retardant effect. The silicon element promotes the carbonization of combustion products and forms a stable The carbonaceous layer prevents oxygen from entering and achieves flame retardant effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004963043710000071
    Figure BDA0004963043710000071
Patent Text Reader

Abstract

The invention relates to the technical field of composite materials, and discloses a high-flame-retardant polypropylene composite material and a preparation method thereof.The high-flame-retardant polypropylene composite material is obtained by adding benzyl chloride-based chitosan, modified carbon nanotubes, silicon-modified boric acid and polypropylene into a double-screw extruder and conducting blending and extrusion. Wherein benzyl chloride in the benzyl chloride-based chitosan reacts with tertiary amine in the modified carbon nanotube and the silicon-modified boric acid to generate a quaternary ammonium salt group with an antibacterial effect. When the polypropylene composite material is combusted, boric acid in the polypropylene composite material can release crystal water and form a glassy coating to cover the surface of the material, so that the flame-retardant effect is achieved, and sulfur and silicon jointly form a flame-retardant system; and the contained carbon nanotubes also have a flame-retardant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, in particular to a high flame retardant polypropylene composite material and a preparation method thereof. Background Art

[0002] Polypropylene is a non-toxic plastic with low price and good processing performance, but it is flammable and has dripping during the combustion process, which limits its use; when exposed to the air for a long time, it will be eroded by bacteria, thus affecting its normal use. Therefore, how to avoid these phenomena is the key to solving the problem. Chitosan has good biodegradability and biocompatibility. The molecular skeleton contains a certain number of side chain groups such as hydroxyl and amino groups. These groups can be carbonized in the polymer during the thermal decomposition process to form a barrier that hinders combustion, thereby playing a flame retardant role. It is applied in the material of the present invention as one of the additives to improve the flame retardant properties of the material. For example, patent CN116041847A discloses a high thermal conductivity flame retardant polypropylene composite material and its preparation method. The composite material has good flame retardant properties, but its antibacterial properties are not improved. Summary of the invention

[0003] 1. Technical issues to be solved

[0004] In view of the deficiencies in the prior art, the present invention provides a highly flame-retardant polypropylene composite material and a preparation method thereof, which has good flame-retardant and antibacterial effects.

[0005] (II) Technical solution

[0006] To achieve the above object, the present invention provides the following technical solution: a highly flame-retardant polypropylene composite material, comprising the following components by weight: 3-5 parts by weight of benzyl chloride chitosan, 4-6 parts by weight of modified carbon nanotubes, 5-8 parts by weight of silicon-modified boric acid, and 60-80 parts by weight of polypropylene.

[0007] Preferably, the preparation method of the silicon-modified boric acid is:

[0008] (1) Add 5-formyl-2-thiopheneboronic acid and pentaerythritol methyl silicate to N,N-dimethylformamide solvent, stir to dissolve, react at 75-85° C. for 10-14 hours, and then distill under reduced pressure, filter and dry to obtain intermediate 1;

[0009] (2) Add 5-aminoisophthalic acid and thionyl chloride to xylene solvent, heat to 65-80° C., reflux for 6-8 hours, and remove the solvent by distillation under reduced pressure to obtain intermediate 2;

[0010] (3) adding intermediate 2 and 4-methyl-5-thiazoleethanol to N,N-dimethylformamide solvent, stirring and mixing, continuing to add pyridine catalyst, reacting at 70-90° C. for 10-12 hours, rotating to remove the solvent after completion, washing with petroleum ether, and drying to obtain sulfur-containing boric acid;

[0011] (4) Add sulfur-containing boric acid and intermediate 1 to an ethanol solvent, react at 70-95° C. for 7-10 h, then add hydrogen-containing silicone oil, react at 65-85° C. for 8-14 h, and then distill under reduced pressure, wash with petroleum ether, and dry to obtain silicon-modified boric acid.

[0012] Preferably, the mass ratio of 5-formyl-2-thiopheneboronic acid to pentaerythritol methyl silicate in (1) is 1:1.6-2.1.

[0013] Preferably, the mass ratio of 5-aminoisophthalic acid to thionyl chloride in (2) is 1:2.5-3.

[0014] Preferably, the mass ratio of the intermediate 2, 4-methyl-5-thiazoleethanol and pyridine catalyst in (3) is 1.1-1.3:1:0.02-0.03.

[0015] Preferably, the mass ratio of sulfur-containing boric acid, intermediate 1, and hydrogen-containing silicone oil in (4) is 1.2-1.4:1:0.8-1.2.

[0016] Preferably, the preparation method of the modified carbon nanotubes is:

[0017] S1. Add 5-8 parts by weight of sulfur-containing boric acid, 6-10 parts by weight of acryloyl chloride and 0.4-0.6 parts by weight of pyridine catalyst to a reaction kettle filled with ether solvent at 0-2°C, introduce nitrogen protection, react at 25-40°C for 6-8h, wash and dry after completion to obtain olefinated boronic acid;

[0018] S2. Add 7-10 parts by weight of olefinated boric acid, 3-5 parts by weight of vinyl carbon nanotubes and 6-12 parts by weight of propylene to N,N-dimethylformamide solvent for dissolution, add 0.4-0.7 parts by weight of azobisisobutyronitrile initiator after dissolution, react at 60-80°C for 2-6h, remove the solvent by distillation under reduced pressure after the reaction, filter, wash and dry to obtain modified carbon nanotubes.

[0019] Preferably, the preparation method of the highly flame-retardant polypropylene composite material is: adding benzyl chloride chitosan, modified carbon nanotubes, silicon-modified boric acid, and polypropylene into a twin-screw extruder, with a blending temperature of 185-190° C. and an extrusion temperature of 170-180° C. to obtain a highly flame-retardant polypropylene composite material.

[0020] (III) Beneficial technical effects

[0021] The invention provides a high flame retardant polypropylene composite material by adding benzyl chloride chitosan, modified carbon nanotubes, silicon-modified boric acid and polypropylene into a twin-screw extruder, blending and extruding. Benzyl chloride in the benzyl chloride chitosan reacts with tertiary amines in the modified carbon nanotubes and silicon-modified boric acid to generate quaternary ammonium salt groups with antibacterial effects.

[0022] The boronic acid group in 5-aldehyde-2-thiopheneboronic acid reacts with the hydroxyl group in pentaerythritol methyl silicate to introduce an aldehyde group, thereby obtaining intermediate 1; the carboxyl group in 5-aminoisophthalic acid reacts with thionyl chloride to introduce an acyl chloride group, which is then reacted with the hydroxyl group in 4-methyl-5-thiazoleethanol to introduce an amino group, thereby obtaining sulfur-containing boronic acid; the amino group in the sulfur-containing boronic acid reacts with the aldehyde group in intermediate 1 to introduce a double bond, which is then subjected to an addition reaction with hydrogen-containing silicone oil to obtain silicon-modified boronic acid.

[0023] When the polypropylene composite material burns, the boric acid in it will release crystal water and form a glass-like coating covering the surface of the material, which plays a role in isolating the air and cooling down, thereby achieving a flame retardant effect. The sulfur element can release strong acids such as sulfuric acid under high temperature conditions. These strong acids can promote the dehydration of the substrate into carbon. The formed carbon layer has the function of heat insulation and air isolation, thereby preventing it from burning; the silicon element can promote the carbonization of combustion products, forming a stable carbonaceous layer, preventing oxygen from entering, and achieving a flame retardant effect; the carbon nanotubes contained therein themselves also have a flame retardant effect. DETAILED DESCRIPTION

[0024] The preparation process of vinyl carbon nanotubes refers to the journal "Materials Science and Engineering Plastics" Volume 23, Issue 4, "Surface Vinyl Functionalization of Multi-walled Carbon Nanotubes": 0.3g of multi-walled carbon nanotubes were added to 30mL of 98% concentrated sulfuric acid and 10mL of 70% concentrated nitric acid, refluxed at 140°C for 1h, filtered, and washed. 0.1g of the acidified carbon nanotubes obtained were weighed and dispersed in 15mL of acetone and 15mL of chloroform, 2mL of triethylamine and 5mL of acryloyl chloride were added, and the reaction was carried out at 40°C for 24h. Then 10mL of ethanol was added, stirred for 2h, filtered, and washed to obtain vinyl carbon nanotubes.

[0025] Add 1 g of chitosan, 0.2 g of 4-chloromethylbenzoyl chloride and 0.4 g of triethylamine to N,N-dimethylformamide, heat to 60°C and stir to react for 36 hours. After the reaction, add distilled water to precipitate, filter the solvent, wash and purify with distilled water and acetone to obtain benzyl chloride chitosan.

[0026] Example 1

[0027] (1) adding 5-formyl-2-thiopheneboronic acid and pentaerythritol methyl silicate to N,N-dimethylformamide solvent, wherein the mass ratio of 5-formyl-2-thiopheneboronic acid to pentaerythritol methyl silicate is 1:1.6, stirring and dissolving, reacting at 75° C. for 10 h, and then distilling under reduced pressure, filtering and drying to obtain intermediate 1;

[0028] (2) adding 5-aminoisophthalic acid and thionyl chloride to a xylene solvent, wherein the mass ratio of 5-aminoisophthalic acid to thionyl chloride is 1:2.5, heating to 65° C., reflux reaction for h, and removing the solvent by distillation under reduced pressure to obtain intermediate 2;

[0029] (3) adding intermediate 2 and 4-methyl-5-thiazoleethanol to N,N-dimethylformamide solvent, stirring and mixing, and continuing to add pyridine catalyst thereto, wherein the mass ratio of intermediate 2, 4-methyl-5-thiazoleethanol, and pyridine catalyst is 1.1:1:0.02, reacting at 70° C. for 10 h, rotating to remove the solvent after completion, washing with petroleum ether, and drying to obtain sulfur-containing boric acid;

[0030] (4) adding sulfur-containing boric acid and intermediate 1 to an ethanol solvent, reacting at 70° C. for 7 h, then adding hydrogenated silicone oil, wherein the mass ratio of sulfur-containing boric acid, intermediate 1, and hydrogenated silicone oil is 1.2:1:0.8, reacting at 65° C. for 8 h, and then distilling under reduced pressure, washing with petroleum ether, and drying to obtain silicon-modified boric acid;

[0031] (5) adding 5 parts by weight of sulfur-containing boric acid, 6 parts by weight of acryloyl chloride and 0.4 parts by weight of pyridine catalyst to a reaction kettle filled with ether solvent at 0° C., introducing nitrogen protection, reacting at 25° C. for 6 h, washing after completion, and drying to obtain olefinated boronic acid;

[0032] (6) adding 7 parts by weight of olefinated boric acid, 3 parts by weight of vinyl carbon nanotubes and 6 parts by weight of propylene to N,N-dimethylformamide solvent for dissolution, adding 0.4 parts by weight of azobisisobutyronitrile initiator after dissolution, reacting at 60° C. for 2 h, removing the solvent by reduced pressure distillation after the reaction, filtering, washing and drying to obtain modified carbon nanotubes;

[0033] (7) 3 parts by weight of benzyl chloride chitosan, 4 parts by weight of modified carbon nanotubes, 5 parts by weight of silicon-modified boric acid, and 60 parts by weight of polypropylene are added into a twin-screw extruder at a blending temperature of 185° C. and an extrusion temperature of 170° C. to obtain a highly flame-retardant polypropylene composite material.

[0034] Example 2

[0035] (1) adding 5-formyl-2-thiopheneboronic acid and pentaerythritol methyl silicate to N,N-dimethylformamide solvent, wherein the mass ratio of 5-formyl-2-thiopheneboronic acid to pentaerythritol methyl silicate is 1:2.1, stirring and dissolving, reacting at 85° C. for 14 h, and then distilling under reduced pressure, filtering and drying to obtain intermediate 1;

[0036] (2) adding 5-aminoisophthalic acid and thionyl chloride to a xylene solvent, wherein the mass ratio of 5-aminoisophthalic acid to thionyl chloride is 1:3, heating to 80° C., reflux reaction for 8 h, and removing the solvent by distillation under reduced pressure to obtain intermediate 2;

[0037] (3) adding intermediate 2 and 4-methyl-5-thiazoleethanol to N,N-dimethylformamide solvent, stirring and mixing, and continuing to add pyridine catalyst thereto, wherein the mass ratio of intermediate 2, 4-methyl-5-thiazoleethanol, and pyridine catalyst is 1.3:1:0.03, reacting at 90° C. for 12 h, rotating to remove the solvent after completion, washing with petroleum ether, and drying to obtain sulfur-containing boric acid;

[0038] (4) adding sulfur-containing boric acid and intermediate 1 to an ethanol solvent, reacting at 95° C. for 10 h, then adding hydrogenated silicone oil, wherein the mass ratio of sulfur-containing boric acid, intermediate 1, and hydrogenated silicone oil is 1.4:1:1.2, reacting at 85° C. for 14 h, and then distilling under reduced pressure, washing with petroleum ether, and drying to obtain silicon-modified boric acid;

[0039] (5) adding 8 parts by weight of sulfur-containing boric acid, 10 parts by weight of acryloyl chloride and 0.6 parts by weight of pyridine catalyst to a reaction kettle filled with ether solvent at 2° C., introducing nitrogen protection, reacting at 40° C. for 8 h, washing after completion, and drying to obtain olefinated boronic acid;

[0040] (6) adding 10 parts by weight of olefinated boric acid, 5 parts by weight of vinyl carbon nanotubes and 12 parts by weight of propylene to N,N-dimethylformamide solvent for dissolution, adding 0.7 parts by weight of azobisisobutyronitrile initiator after dissolution, reacting at 80° C. for 6 hours, removing the solvent by reduced pressure distillation after the reaction, filtering, washing and drying to obtain modified carbon nanotubes;

[0041] (7) 5 parts by weight of benzyl chloride chitosan, 6 parts by weight of modified carbon nanotubes, 5-8 parts by weight of silicon-modified boric acid, and 80 parts by weight of polypropylene are added into a twin-screw extruder at a blending temperature of 190° C. and an extrusion temperature of 180° C. to obtain a highly flame-retardant polypropylene composite material.

[0042] Example 3

[0043] (1) adding 5-formyl-2-thiopheneboronic acid and pentaerythritol methyl silicate to N,N-dimethylformamide solvent, wherein the mass ratio of 5-formyl-2-thiopheneboronic acid to pentaerythritol methyl silicate is 1:1.85, stirring and dissolving, reacting at 80° C. for 12 h, and then distilling under reduced pressure, filtering and drying to obtain intermediate 1;

[0044] (2) adding 5-aminoisophthalic acid and thionyl chloride to a xylene solvent, wherein the mass ratio of 5-aminoisophthalic acid to thionyl chloride is 1:2.75, heating to 72° C., reflux reaction for 7 h, and removing the solvent by distillation under reduced pressure to obtain intermediate 2;

[0045] (3) adding intermediate 2 and 4-methyl-5-thiazoleethanol to N,N-dimethylformamide solvent, stirring and mixing, and continuing to add pyridine catalyst thereto, wherein the mass ratio of intermediate 2, 4-methyl-5-thiazoleethanol, and pyridine catalyst is 1.2:1:0.025, reacting at 80° C. for 11 h, rotating to remove the solvent after completion, washing with petroleum ether, and drying to obtain sulfur-containing boric acid;

[0046] (4) adding sulfur-containing boric acid and intermediate 1 to an ethanol solvent, reacting at 82° C. for 8.5 h, then adding hydrogenated silicone oil, wherein the mass ratio of sulfur-containing boric acid, intermediate 1, and hydrogenated silicone oil is 1.3:1:1, reacting at 75° C. for 11 h, and then distilling under reduced pressure, washing with petroleum ether, and drying to obtain silicon-modified boric acid;

[0047] (5) adding 6.5 parts by weight of sulfur-containing boric acid, 8 parts by weight of acryloyl chloride and 0.5 parts by weight of pyridine catalyst to a reaction kettle filled with ether solvent at 1° C., introducing nitrogen protection, reacting at 32.5° C. for 7 h, washing and drying after the reaction to obtain olefinated boronic acid;

[0048] (6) adding 8.5 parts by weight of olefinated boric acid, 4 parts by weight of vinyl carbon nanotubes and 9 parts by weight of propylene to N,N-dimethylformamide solvent for dissolution, adding 0.55 parts by weight of azobisisobutyronitrile initiator after dissolution, reacting at 70° C. for 4 hours, and removing the solvent by reduced pressure distillation after the reaction, filtering, washing and drying to obtain modified carbon nanotubes;

[0049] (7) 4 parts by weight of benzyl chloride chitosan, 5 parts by weight of modified carbon nanotubes, 6.5 parts by weight of silicon-modified boric acid, and 70 parts by weight of polypropylene are added into a twin-screw extruder at a blending temperature of 187.5° C. and an extrusion temperature of 175° C. to obtain a highly flame-retardant polypropylene composite material.

[0050] Comparative Example 1

[0051] (1) 4 parts by weight of benzyl chloride chitosan, 6.5 parts by weight of silicon-modified boric acid, and 70 parts by weight of polypropylene are added into a twin-screw extruder at a blending temperature of 187.5° C. and an extrusion temperature of 175° C. to obtain a highly flame-retardant polypropylene composite material.

[0052] Comparative Example 2

[0053] (1) 4 parts by weight of benzyl chloride chitosan, 5 parts by weight of modified carbon nanotubes, and 70 parts by weight of polypropylene are added into a twin-screw extruder at a blending temperature of 187.5° C. and an extrusion temperature of 175° C. to obtain a highly flame-retardant polypropylene composite material.

[0054] Use an oxygen index meter to test the limiting oxygen index of the adhesive; use a horizontal and vertical combustion instrument to test the combustion level of the adhesive.

[0055] Table 1: Tests of flame retardancy.

[0056]

[0057]

[0058] It can be seen from Table 1 that the highly flame-retardant polypropylene composite materials prepared in Examples 1-3 of the present invention have better flame-retardant effects than those prepared in Comparative Examples 1-2;

[0059] The highly flame-retardant polypropylene composite material was dissolved and cast into a film to make a thin sheet with a radius of 1 cm; then the bacteria were transferred to a sterile culture medium using an inoculation loop to culture the bacteria at a concentration of 10 6 CFU / mL of bacterial suspension, then transfer 0.5mL of the bacterial suspension to a culture dish containing beef extract peptone medium, shake evenly, add chitosan slices, and culture in a constant temperature incubator. After 48 hours of culture, measure the diameter of the inhibition zone.

[0060] Table 2: Inhibition zones / mm for different bacteria.

[0061] sample Escherichia coli (mm) Staphylococcus aureus (mm) Example 1 13.9 14.7 Example 2 18.7 16.5 Example 3 17.5 15.3 Comparative Example 1 6.4 7.9 Comparative Example 2 6.5 7.2

[0062] It can be seen from Table 2 that the highly flame-retardant polypropylene composite materials prepared in Examples 1-3 of the present invention have better antibacterial effects than those prepared in Comparative Examples 1-2.

[0063] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A highly flame-retardant polypropylene composite material, characterized in that: The invention comprises the following components by weight: 3-5 parts by weight of benzyl chloride chitosan, 4-6 parts by weight of modified carbon nanotubes, 5-8 parts by weight of silicon-modified boric acid and 60-80 parts by weight of polypropylene.

2. The highly flame-retardant polypropylene composite material according to claim 1, characterized in that: The preparation method of the silicon-modified boric acid is: (1) Add 5-formyl-2-thiopheneboronic acid and pentaerythritol methyl silicate to N,N-dimethylformamide solvent, stir to dissolve, react at 75-85° C. for 10-14 hours, and then distill under reduced pressure, filter and dry to obtain intermediate 1; (2) Add 5-aminoisophthalic acid and thionyl chloride to xylene solvent, heat to 65-80° C., reflux for 6-8 hours, and remove the solvent by distillation under reduced pressure to obtain intermediate 2; (3) adding intermediate 2 and 4-methyl-5-thiazoleethanol to N,N-dimethylformamide solvent, stirring and mixing, continuing to add pyridine catalyst, reacting at 70-90° C. for 10-12 hours, rotating to remove the solvent after completion, washing with petroleum ether, and drying to obtain sulfur-containing boric acid; (4) Add sulfur-containing boric acid and intermediate 1 to an ethanol solvent, react at 70-95° C. for 7-10 h, then add hydrogen-containing silicone oil, react at 65-85° C. for 8-14 h, and then distill under reduced pressure, wash with petroleum ether, and dry to obtain silicon-modified boric acid.

3. The highly flame-retardant polypropylene composite material according to claim 2, characterized in that: The mass ratio of 5-formyl-2-thiopheneboronic acid to pentaerythritol methyl silicate in (1) is 1:1.6-2.

1.

4. The highly flame-retardant polypropylene composite material according to claim 2, characterized in that: The mass ratio of 5-aminoisophthalic acid to thionyl chloride in (2) is 1:2.5-3.

5. The highly flame-retardant polypropylene composite material according to claim 2, characterized in that: The mass ratio of the intermediate 2, 4-methyl-5-thiazoleethanol and pyridine catalyst in (3) is 1.1-1.3:1:0.02-0.

03.

6. The highly flame-retardant polypropylene composite material according to claim 2, characterized in that: The mass ratio of sulfur-containing boric acid, intermediate 1, and hydrogen-containing silicone oil in (4) is 1.2-1.4:1:0.8-1.

2.

7. The highly flame-retardant polypropylene composite material according to claim 1, characterized in that: The preparation method of the modified carbon nanotubes is: S1. Add 5-8 parts by weight of sulfur-containing boric acid, 6-10 parts by weight of acryloyl chloride and 0.4-0.6 parts by weight of pyridine catalyst to a reaction kettle filled with ether solvent at 0-2°C, introduce nitrogen protection, react at 25-40°C for 6-8h, wash and dry after completion to obtain olefinated boronic acid; S2. Add 7-10 parts by weight of olefinated boric acid, 3-5 parts by weight of vinyl carbon nanotubes and 6-12 parts by weight of propylene to N,N-dimethylformamide solvent for dissolution, add 0.4-0.7 parts by weight of azobisisobutyronitrile initiator after dissolution, react at 60-80°C for 2-6h, remove the solvent by distillation under reduced pressure after the reaction, filter, wash and dry to obtain modified carbon nanotubes.

8. A method for preparing a highly flame-retardant polypropylene composite material according to any one of claims 1 to 7, characterized in that: The preparation method of the high flame retardant polypropylene composite material is as follows: benzyl chloride chitosan, modified carbon nanotubes, silicon-modified boric acid and polypropylene are added into a twin-screw extruder, the blending temperature is 185-190° C., the extrusion temperature is 170-180° C., and the high flame retardant polypropylene composite material is obtained.

Citation Information

Cited By

  • Antibacterial chitosan grafted polypropylene composite film and preparation method thereof

    CN119391020A

  • Corrosion-resistant polypropylene edge band material and preparation method thereof

    CN119823494A

  • Corrosion-resistant polypropylene edge strip material and method of making same

    CN119823494B