Polypropylene polyol resin
Through the preparation of polypropylene polyol resin, the use of microwave activation of polypropylene double bonds to form a stable three-dimensional interlaced space structure, solving the problems of low domestic production rate and high cost of fluoroelastomer in power battery sealing rings, achieving high mechanical properties and low water absorption The sealing ring material is replaced by type 246 peroxide fluoroelastomer and reduces the raw material cost.
Patent Information
- Application Number
- CN202411104231.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The domestic production rate of fluoroelastomer of the power battery sealing ring is low and the price is high, which affects the leakage and explosion safety performance of the battery and has an impact on the overall performance of the discharge capacity.
Polypropylene polyol resin is prepared from raw materials such as polypropylene powder, hydrogenated rosin resin, disproportionate rosin and fillers. After dynamic cross-linking through a double-roll granulator, double bonds are activated under microwaves to form a stable three-dimensional interlaced space structure. It provides sealing ring materials with high mechanical properties, low water absorption, high temperature and corrosion resistance.
The prepared polypropylene polyol resin sealing ring material has a performance of close to that of type 246 peroxide fluoroelastomer, which can replace type 246 peroxide fluoroelastomer in most fields, and the raw material cost is lower, making it easier to promote.
Smart Images

Figure CN118931035A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealing rings, in particular to a polypropylene polyol resin. Background Art
[0002] The battery sealing ring plays a decisive role in the leak-proof and explosion-proof safety performance of the battery, and also affects the overall performance of the battery discharge capacity.
[0003] The sealing ring of power batteries is an important safety component of the battery, and is mainly made of fluororubber. The low localization rate and high price of fluororubber have always been a pain point in the power battery sealing industry. Summary of the invention
[0004] The present invention provides a polypropylene polyol resin to solve the problems raised in the above background technology.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A polypropylene polyol resin is prepared from the following raw materials in parts by weight: 60-70 parts of polypropylene powder, 20-30 parts of hydrogenated rosin resin, 10-20 parts of disproportionated rosin, 5-10 parts of filler, and 1-5 parts of oxidant;
[0007] The preparation method of the polypropylene polyol resin is:
[0008] S1, first adding polypropylene powder and filler in a double-roll granulator according to weight proportions, then adding hydrogenated rosin resin and disproportionated rosin, and then adding an oxidant for dynamic crosslinking and granulation;
[0009] S2, the prepared pellets are further subjected to microwave irradiation at a specific power of 12-15KW. When high-energy microwaves at a power of 12-15KW pass through the pellets, double bonds in the pellets are activated to generate macromolecular free radicals. A large number of free radicals combine with each other to form a stable three-dimensional staggered spatial structure of the macromolecules, thereby obtaining polypropylene polyol resin.
[0010] As a further improvement of the technical solution: the granulation temperature of the double-roll granulator is between 180-210 degrees.
[0011] As a further improvement of the present technical solution: hydrogenated rosin resin includes but is not limited to: hydrogenated rosin glycerol resin, hydrogenated rosin pentaerythritol resin and hydrogenated rosin phenolic resin.
[0012] As a further improvement of the present technical solution: the disproportionated rosin includes dihydroabietic acid and tetrahydroabietic acid.
[0013] As a further improvement of the technical solution: the filler includes but is not limited to nano silicon dioxide powder, nano barium sulfate and molybdenum disulfide.
[0014] As a further improvement of the present technical solution: the oxidant includes but is not limited to DCP, TAIC and hydrogen peroxide.
[0015] As a further improvement of the technical solution: the crystallinity of the polypropylene polyol resin is above 40%.
[0016] As a further improvement of the technical solution: it is prepared from the following raw materials in parts by weight: 60 parts of polypropylene powder, 20 parts of hydrogenated rosin resin, 10 parts of disproportionated rosin, 5 parts of filler, and 1 part of oxidant.
[0017] As a further improvement of the technical solution: it is prepared from the following raw materials in parts by weight: 65 parts of polypropylene powder, 25 parts of hydrogenated rosin resin, 15 parts of disproportionated rosin, 8 parts of filler, and 3 parts of oxidant.
[0018] As a further improvement of the technical solution: it is prepared from the following raw materials in parts by weight: 70 parts of polypropylene powder, 30 parts of hydrogenated rosin resin, 20 parts of disproportionated rosin, 10 parts of filler, and 5 parts of oxidant.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The polypropylene polyol resin proposed by the present invention is obtained by activating the double bonds of polypropylene by microwave irradiation, so that the triphenyl ring structure and the double bonds of polypropylene are fully cross-linked to form a stable and elastic three-dimensional staggered space structure. This structure has strong stability and can resist the impact of most chemical bonds and physical bonds, so that the prepared polypropylene polyol resin sealing ring material not only has good mechanical properties, but also has low water absorption, high temperature resistance and corrosion resistance.
[0021] The performance of this polypropylene polyol resin product is close to that of 246-type peroxy fluororubber, and it can replace 246-type peroxy fluororubber in most fields. In addition, the cost of related raw materials of this product is lower, which is easy to promote.
[0022] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. The specific implementation of the present invention is given in detail by the following embodiments and their accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0024] Figure 1 The present invention provides a schematic diagram of the steps of preparing a polypropylene polyol resin. DETAILED DESCRIPTION
[0025] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention. The present invention is described in more detail by way of example with reference to the accompanying drawings in the following paragraphs. It should be noted that the accompanying drawings are all in a very simplified form and are not in precise proportions, and are only used to facilitate and clearly assist in explaining the purpose of the embodiments of the present invention.
[0026] Embodiment 1
[0027] A polypropylene polyol resin is prepared from the following raw materials in parts by weight: 60 parts of polypropylene powder, 20 parts of hydrogenated rosin resin, 10 parts of disproportionated rosin, 5 parts of filler, and 1 part of oxidant;
[0028] The preparation method of the polypropylene polyol resin is:
[0029] S1, first add polypropylene powder and filler in a double-roll granulator according to weight proportions, then add hydrogenated rosin resin and disproportionated rosin, then add an oxidant for dynamic crosslinking and granulation, the granulation temperature of the double-roll granulator is between 180-210 degrees;
[0030] Hydrogenated rosin resins include but are not limited to: hydrogenated rosin glycerol resin, hydrogenated rosin pentaerythritol resin and hydrogenated rosin phenolic resin;
[0031] Disproportionated rosin includes dihydroabietic acid and tetrahydroabietic acid;
[0032] Fillers include but are not limited to nano silicon dioxide powder, nano barium sulfate and molybdenum disulfide;
[0033] Oxidants include but are not limited to DCP, TAIC and hydrogen peroxide;
[0034] S2, the prepared pellets are further subjected to microwave irradiation at a specific power of 12-15KW. When the high-energy microwaves at a power of 12-15KW pass through the pellets, the double bonds in the pellets are activated to generate macromolecular free radicals. A large number of free radicals combine with each other to form a stable three-dimensional staggered spatial structure of the macromolecules, thereby obtaining a polypropylene polyol resin having a crystallinity of more than 40%.
[0035] Embodiment 2
[0036] The technical feature that distinguishes Example 2 from Example 1 is: a polypropylene polyol resin is prepared from the following raw materials in parts by weight: 65 parts of polypropylene powder, 25 parts of hydrogenated rosin resin, 15 parts of disproportionated rosin, 8 parts of filler, and 3 parts of oxidant.
[0037] Embodiment 3
[0038] The technical feature that distinguishes Example 3 from Example 1 is: a polypropylene polyol resin is prepared from the following raw materials in parts by weight: 70 parts of polypropylene powder, 30 parts of hydrogenated rosin resin, 20 parts of disproportionated rosin, 10 parts of filler, and 5 parts of oxidant.
[0039] The polypropylene polyol resins obtained in Examples 1, 2 and 3 were dried in an oven at 120° C. for 2 h and then injection molded into sealing rings of the same size using an injection molding machine. The following properties were tested respectively:
[0040] 1. Tensile strength: Tested according to ASTMD638 standard
[0041] 2. Water absorption rate: According to ASTM D570-2005 plastic water absorption test method, soak at 23 ° C for 24 hours and test the water absorption rate (%);
[0042] 3. Heat deformation temperature: Use method B in the standard test method for deformation temperature of plastics under side vertical bending load in ASTM D648-04, with a heating rate of 120℃ / h and a load of 1.85MPa to test the heat deformation temperature (℃);
[0043] 4. Corrosion resistance: Place the sample in 98% HNO3 and immerse it at room temperature for 30 days. Test the volume expansion rate (%) of the sample.
[0044] The test results are shown in the following table:
[0045] Embodiment 1 Embodiment 2 Embodiment 3 Tensile strength(MPa) 147 151 162 Water absorption (%) 0.9 1.0 0.9 Heat deformation temperature(℃) 98 95 96 Volume expansion rate (%) 8.7 9.2 8.9
[0046] As can be seen from the above table, since the abietic acid in the hydrogenated rosin resin and the disproportionated rosin has a unique triphenyl ring structure, a unique spatial structure is formed, and the triphenyl ring structure can be cross-linked with double bonds and carboxyl groups. When the resin is irradiated with microwaves, the polypropylene double bonds can be activated to generate macromolecular free radicals, and the free radicals allow the triphenyl ring structure and the double bonds of polypropylene to fully cross-link, forming a stable and elastic three-dimensional staggered spatial structure, which has strong stability and can resist the impact of most chemical bonds and physical bonds. Therefore, the polypropylene polyol resin sealing ring material prepared in Examples 1, 2, and 3 not only has good mechanical properties, but also has low water absorption, high temperature resistance, and corrosion resistance.
[0047] The performance of this product is close to that of 246 type peroxy fluororubber, and it can replace 246 type peroxy fluororubber in most fields. In addition, the cost of related raw materials of this product is lower, which is easy to promote.
[0048] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as shown in the drawings and described above. However, any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. A polypropylene polyol resin, characterized in that The invention is prepared from the following raw materials in parts by weight: 60-70 parts of polypropylene powder, 20-30 parts of hydrogenated rosin resin, 10-20 parts of disproportionated rosin, 5-10 parts of filler, and 1-5 parts of oxidant; The preparation method of the polypropylene polyol resin is: S1, first adding polypropylene powder and filler in a double-roll granulator according to weight proportions, then adding hydrogenated rosin resin and disproportionated rosin, and then adding an oxidant for dynamic crosslinking and granulation; S2, the prepared pellets are further subjected to microwave irradiation at a specific power of 12-15KW. When high-energy microwaves at a power of 12-15KW pass through the pellets, double bonds in the pellets are activated to generate macromolecular free radicals. A large number of free radicals combine with each other to form a stable three-dimensional staggered spatial structure of the macromolecules, thereby obtaining polypropylene polyol resin.
2. A polypropylene polyol resin according to claim 1, characterized in that, The granulation temperature of the double-roll granulator is between 180 and 210 degrees.
3. A polypropylene polyol resin according to claim 1, characterized in that, The hydrogenated rosin resin includes, but is not limited to, hydrogenated rosin glycerol resin, hydrogenated rosin pentaerythritol resin, and hydrogenated rosin phenolic resin.
4. A polypropylene polyol resin according to claim 1, characterized in that, Disproportionated rosin includes dihydroabietic acid and tetrahydroabietic acid.
5. A polypropylene polyol resin according to claim 1, characterized in that: The fillers include but are not limited to nano silicon dioxide powder, nano barium sulfate and molybdenum disulfide.
6. A polypropylene polyol resin according to claim 1, characterized in that: Oxidants include but are not limited to DCP, TAIC and hydrogen peroxide.
7. A polypropylene polyol resin according to claim 1, characterized in that: The crystallinity of the polypropylene polyol resin is above 40%.
8. A polypropylene polyol resin according to claim 1, characterized in that: The invention is prepared from the following raw materials in parts by weight: 60 parts of polypropylene powder, 20 parts of hydrogenated rosin resin, 10 parts of disproportionated rosin, 5 parts of filler and 1 part of oxidant.
9. A polypropylene polyol resin according to claim 1, characterized in that: The invention is prepared from the following raw materials in parts by weight: 65 parts of polypropylene powder, 25 parts of hydrogenated rosin resin, 15 parts of disproportionated rosin, 8 parts of filler and 3 parts of oxidant.
10. A polypropylene polyol resin according to claim 1, characterized in that: The invention is prepared from the following raw materials in parts by weight: 70 parts of polypropylene powder, 30 parts of hydrogenated rosin resin, 20 parts of disproportionated rosin, 10 parts of filler and 5 parts of oxidant.