Plasma-treatment-free glass fiber reinforced polypropylene material and preparation method thereof
By using modified glass fibers in polypropylene materials, dopamine and hyperbranched polyetheramine polymers are used to improve the surface polarity of the material, solving the problem of plasma treatment when existing polypropylene materials are covered, and achieving mechanical properties Improve and save costs.
Patent Information
- Application Number
- CN202411104477.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
Existing polypropylene materials require plasma treatment when surface coating, which increases production processes and costs, and the surface polarity is not sufficient to meet certain application requirements.
By adding dopamine hydrochloride aqueous solution to the glass fibers, polydopamine is coated, and the hyperbranched polyetheramine polymer is reacted with it to form modified glass fibers, combining polypropylene, compatible agents, and antioxidants. and lubricant, a plasma-free glass fiber reinforced polypropylene material with improved surface polarity was prepared.
The mechanical properties and surface polarity of the modified polypropylene material are significantly improved, reaching more than 42dyn, avoiding plasma treatment processes, and saving production processes and costs.
Smart Images

Figure CN118931036A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a plasma-free glass fiber reinforced polypropylene material and a preparation method thereof. Background Art
[0002] Polypropylene (PP) is a thermoplastic resin and one of the five most common plastics. Its density is only 0.90g / cm 3 , is the lightest general-purpose plastic. It has the advantages of good chemical stability, mechanical properties, good molding and processing performance and low price, and has been widely used in the fields of automobiles, chemicals, stationery, electrical appliances, construction, experimental instruments, etc. By using the glass fiber reinforcement modification method, a polypropylene composite material with high modulus, high strength, high heat resistance and good dimensional stability can be prepared, which is widely used in products such as automobile instrument panels and auxiliary instrument panel frames. Due to the low surface activation energy of PP and poor surface polarity, when soft instrument panels or auxiliary instruments are coated, the glass fiber modified polypropylene material needs to be subjected to surface plasma treatment, and the surface polarity reaches more than 40dyn to meet the requirements of PVC and other surface coatings. Summary of the invention
[0003] In view of the deficiencies in the prior art, the present invention provides a plasma-free glass fiber reinforced polypropylene material and a preparation method thereof.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] The first aspect of the present invention relates to a plasma-free glass fiber reinforced polypropylene material, comprising the following raw materials in parts by weight:
[0006] Polypropylene 65-85 parts, modified glass fiber 20-30 parts, compatibilizer 2-6 parts, antioxidant 0.2-0.6 parts and lubricant 0.3-0.8 parts;
[0007] The preparation method of the modified glass fiber comprises the following steps:
[0008] Adding dopamine hydrochloride aqueous solution and glass fiber into a reaction kettle, mixing, introducing oxygen to carry out oxidative polymerization reaction, and obtaining polydopamine coated glass fiber;
[0009] The ethanol solution of polyethylene glycol diglycidyl ether is added dropwise to the ethanol solution of N-ethylethylenediamine, and after the reaction, the hyperbranched polyetheramine polymer is obtained by concentration and precipitation;
[0010] Dopamine hydrochloride is added to the polydopamine coated glass fiber, and then a hyperbranched polyetheramine polymer is added, and after reaction, the modified glass fiber is obtained by filtering and washing.
[0011] Optionally, the compatibilizer is one or more of polypropylene grafted maleic anhydride or polypropylene grafted acrylic acid.
[0012] Optionally, the antioxidant is one or more of antioxidant 1076, antioxidant 1010, antioxidant 1790, antioxidant 626, and antioxidant 168.
[0013] Optionally, the lubricant is one or more of ethylene bisstearamide, pentaerythritol stearate, zinc stearate, and calcium stearate.
[0014] Optionally, it also includes: 1-2 portions of color powder.
[0015] Optionally, the color powder is a PE-based masterbatch.
[0016] Optionally, the polypropylene is a homopolymer or copolymer polypropylene with a melt index between 10-60.
[0017] The second aspect of the present invention relates to a method for preparing a plasma-free glass fiber reinforced polypropylene material, comprising the following steps:
[0018] Adding dopamine hydrochloride aqueous solution and glass fiber into a reaction kettle, mixing, introducing oxygen to carry out oxidative polymerization reaction, and obtaining polydopamine coated glass fiber;
[0019] The ethanol solution of polyethylene glycol diglycidyl ether is added dropwise to the ethanol solution of N-ethylethylenediamine, and after the reaction, the hyperbranched polyetheramine polymer is obtained by concentration and precipitation;
[0020] Adding dopamine hydrochloride to the polydopamine coated glass fiber, and then adding a hyperbranched polyetheramine polymer, filtering and washing after the reaction to obtain the modified glass fiber;
[0021] Put 65-85 parts by weight of polypropylene, 2-6 parts by weight of a compatibilizer, 0.2-0.6 parts by weight of an antioxidant and 0.3-0.8 parts by weight of a lubricant into a high-speed mixer and mix to obtain a mixed material;
[0022] 20-30 parts by weight of modified glass fiber are added into the mixed material from the side feeding system of the extrusion stage, and the mixed material is melted, extruded, granulated and dried to obtain a plasma-free glass fiber reinforced polypropylene material.
[0023] The third aspect of the present invention relates to the use of the above-mentioned plasma-free glass fiber reinforced polypropylene material in the preparation of automobile instrument panels or electrical appliance housings.
[0024] Beneficial effects of the present invention:
[0025] 1. The glass fiber coated with polydopamine has better compatibility with the resin, which can improve the mechanical properties of the modified material and improve the surface floating fiber situation.
[0026] 2. By using glass fiber modified with hyperbranched polyetheramine grafted with polydopamine and utilizing the large number of strong polar groups contained in the hyperbranched polyetheramine chain segments, the polarity of modified polypropylene can be significantly improved, and the surface dyne value can reach more than 42. In the application of coating products, the plasma treatment process can be eliminated, saving production processes and comprehensive costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 These are experimental data of various embodiments and comparative examples of this application. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The specific information of the raw materials used in the examples and comparative examples of the present application is as follows:
[0030] Polypropylene, SZ30S produced by Wuhan Petrochemical;
[0031] Compatibilizer, manufactured by Arkema, France, CA100;
[0032] Antioxidant, manufactured by BASF, brand 1010 or 168;
[0033] Lubricant, manufactured by Kao, Japan, brand P130;
[0034] Toner, manufactured by Cabot, brand number 2718.
[0035] All materials are commercially available common products.
[0036] It is to be understood that the above raw materials and reagents are only examples of some specific embodiments of the present invention, so that the technical solution of the present invention is clearer, and it does not mean that the present invention can only use the above reagents, and the specific scope in the claims shall prevail. In addition, the "parts" described in the examples and comparative examples, unless otherwise specified, refer to parts by weight.
[0037] Among them, the preparation method of the modified glass fiber involved in the embodiments of the present application is as follows:
[0038] Step 1: Add a 1.5 g / L dopamine hydrochloride aqueous solution and glass fiber into a reactor, start the stirrer at a speed of 200 rpm, control the temperature at 30°C and stir for 10 min, then add a Na2CO3 aqueous solution to adjust the pH value to 8-9, introduce oxygen, and perform an oxidative polymerization reaction for 3 h, then filter and wash to obtain polydopamine-coated glass fiber GF-PDA;
[0039] Step 2: Add the ethanol solution of polyethylene glycol diglycidyl ether to the ethanol solution of N-ethylethylenediamine at 0°C, and stir the reaction at room temperature for 48 hours to allow the primary amino group to react fully. Under nitrogen protection, the mixture is refluxed at 80°C for 24 hours. After the reaction is completed, wait for the mixture to cool to room temperature. Concentrate the reaction solution to 15mL by rotary evaporation, and then precipitate in 10 times n-hexane. The product is placed in a vacuum oven at 60°C and dried for 24 hours to obtain a hyperbranched polyetheramine polymer.
[0040] Step 3: Weigh an appropriate amount of the GF-PDA prepared above, add a 5 g / L dopamine hydrochloride aqueous solution, start the stirrer, rotate at 200 rpm, control the temperature at 30 ° C and stir for 10 min, then add the hyperbranched polyetheramine polymer, adjust the pH value to 8-9, react, filter and wash to obtain a modified glass fiber with a GF-PDA-hyperbranched polymer three-layer structure.
[0041] Example 1
[0042] S1. Put 75 parts of polypropylene, 20 parts of modified glass fiber, 2 parts of compatibilizer CA100, 0.2 parts of antioxidants 1010 and 168 (1010 and 168 are in a weight ratio of 3:2), 0.3 parts of lubricant, and 1 part of toner into a high-speed mixer and mix for 5 minutes to obtain a mixed material;
[0043] S2, putting the mixed material of step S1 into a twin-screw extruder, and obtaining modified polypropylene pellets through melting, extrusion, granulation and drying; the barrel temperature of the twin-screw extruder is 190-220° C., and the screw speed is 500 r / min;
[0044] Example 2
[0045] The preparation method is the same as that of Example 1. The raw materials are: 70 parts of polypropylene, 25 parts of modified glass fiber, 4 parts of compatibilizer CA100, 0.4 parts of antioxidants 1010 and 168 (1010 and 168 are in a weight ratio of 3:2), 0.5 parts of lubricant, and 1 part of color powder, which are put into a high-speed mixer and mixed for 5 minutes to obtain a mixed material;
[0046] Example 3
[0047] The preparation method is the same as that of Example 1. The raw materials are: 65 parts of polypropylene, 30 parts of modified glass fiber, 6 parts of compatibilizer CA100, 0.6 parts of antioxidants 1010 and 168 (1010 and 168 are in a weight ratio of 3:2), 0.8 parts of lubricant, and 2 parts of toner, which are put into a high-speed mixer and mixed for 5 minutes to obtain a mixed material;
[0048] Comparative Example 1
[0049] The preparation method is the same as that of Example 1, 65 parts of polypropylene, 30 parts of unmodified glass fiber, 5 parts of compatibilizer, 0.6 parts of antioxidants 1010 and 168 (1010 and 168 according to a weight ratio of 3:2), and 2 parts of toner are put into a high-speed mixer and mixed for 5 minutes to obtain a mixed material;
[0050] Comparative Example 2
[0051] The preparation method is the same as that of Example 1, 75 parts of polypropylene, 20 parts of unmodified glass fiber, 2 parts of compatibilizer, 0.2 parts of antioxidants 1010 and 168 (1010 and 168 according to a weight ratio of 3:2), and 1 part of toner are put into a high-speed mixer and mixed for 5 minutes to obtain a mixed material;
[0052] Comparative Example 3
[0053] The preparation method is the same as that of Example 1, 75 parts of polypropylene, 30 parts of polydopamine coated glass fiber GF-PDA, 6 parts of compatibilizer, 0.6 parts of antioxidants 1010 and 168 (1010 and 168 according to a weight ratio of 3:2), and 2 parts of color powder are put into a high-speed mixer and mixed for 5 minutes to obtain a mixed material;
[0054] In order to demonstrate the technical effect achieved by this technical solution, the following experiment was conducted.
[0055] The polypropylene materials easy to use for water-based paint spraying prepared in Examples 1-6 and the modified polypropylene materials prepared in Comparative Examples 1-3 were injection molded into 500mm*1000mm*3mm samples, and the dyne value of the sample surface was tested according to the standard of Q / CC SY788, and the mechanical properties were tested according to ISO 527 / ISO 178 / ISO 179 for the corresponding tensile, bending and impact properties. The test results are shown in Figure 2. Figure 1 shown.
[0056] From the above test results, it can be seen that the modified polypropylene pellets with different filling ratios in Examples 1-3 have significantly increased surface dyne values and significantly improved mechanical properties. Specifically, by comparing Comparative Examples 1-2 with Examples 1-3, it can be seen that the introduction of modified glass fibers has an improving effect on the mechanical properties of the material. By comparing Example 1 and Comparative Example 3, it can be seen that the glass fibers modified by grafting polydopamine with hyperbranched polyetheramine can significantly improve the surface dyne value of the product.
[0057] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0058] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A plasma-free glass fiber reinforced polypropylene material, characterized in that: It includes the following raw materials in parts by weight: Polypropylene 65-85 parts, modified glass fiber 20-30 parts, compatibilizer 2-6 parts, antioxidant 0.2-0.6 parts and lubricant 0.3-0.8 parts; The preparation method of the modified glass fiber comprises the following steps: Adding dopamine hydrochloride aqueous solution and glass fiber into a reaction kettle, mixing, introducing oxygen to carry out oxidative polymerization reaction, and obtaining polydopamine coated glass fiber; The ethanol solution of polyethylene glycol diglycidyl ether is added dropwise to the ethanol solution of N-ethylethylenediamine, and after the reaction, the hyperbranched polyetheramine polymer is obtained by concentration and precipitation; Dopamine hydrochloride is added to the polydopamine coated glass fiber, and then a hyperbranched polyetheramine polymer is added, and after reaction, the modified glass fiber is obtained by filtering and washing.
2. The plasma-free glass fiber reinforced polypropylene material according to claim 1, characterized in that: The compatibilizer is one or more of polypropylene grafted with maleic anhydride or polypropylene grafted with acrylic acid.
3. The plasma-free glass fiber reinforced polypropylene material according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1076, antioxidant 1010, antioxidant 1790, antioxidant 626, and antioxidant 168.
4. The plasma-free glass fiber reinforced polypropylene material according to claim 1, characterized in that: The lubricant is one or more of ethylene bis stearamide, pentaerythritol stearate, zinc stearate, and calcium stearate.
5. The plasma-free glass fiber reinforced polypropylene material according to claim 1, characterized in that: Also includes: 1-2 parts of color powder.
6. The plasma-free glass fiber reinforced polypropylene material according to claim 5, characterized in that: The color powder is PE-based masterbatch.
7. The plasma-free glass fiber reinforced polypropylene material according to claim 1, characterized in that: The polypropylene is a homopolymer or copolymer polypropylene with a melt index between 10-60.
8. A method for preparing a plasma-free glass fiber reinforced polypropylene material, characterized in that: The following steps are involved: Adding dopamine hydrochloride aqueous solution and glass fiber into a reaction kettle, mixing, introducing oxygen to carry out oxidative polymerization reaction, and obtaining polydopamine coated glass fiber; The ethanol solution of polyethylene glycol diglycidyl ether is added dropwise to the ethanol solution of N-ethylethylenediamine, and after the reaction, the hyperbranched polyetheramine polymer is obtained by concentration and precipitation; Adding dopamine hydrochloride to the polydopamine coated glass fiber, and then adding a hyperbranched polyetheramine polymer, filtering and washing after the reaction to obtain the modified glass fiber; Put 65-85 parts by weight of polypropylene, 2-6 parts by weight of a compatibilizer, 0.2-0.6 parts by weight of an antioxidant and 0.3-0.8 parts by weight of a lubricant into a high-speed mixer and mix to obtain a mixed material; 20-30 parts by weight of modified glass fiber are added into the mixed material from the side feeding system of the extrusion stage, and the mixed material is melted, extruded, granulated and dried to obtain a plasma-free glass fiber reinforced polypropylene material.