Preparation method of EPDM (Ethylene-Propylene-Diene Monomer) insulating rubber sealing strip with low density and good water resistance
Through the combination of two-stage kneading process and specific materials, low-density and good water resistance EPDM seal strips are prepared, which solves the problems of high density and insufficient electrical insulation performance of traditional seal strips, and achieves lightweight design and safety performance improvement.
Patent Information
- Application Number
- CN202411251425.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-07
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional automobile seal strips are dense due to filling in inorganic materials such as kaolin and heavy calcium carbonate, and have a large weight per unit volume, which violates the needs of lightweight design, and lacks electrical insulation performance in new energy vehicles.
The two-stage mixing process is used to prepare low-density, good water resistance EPDM insulating rubber seal strips, using materials such as ethylene propylene ternary rubber, nano-activated calcium carbonate, hollow glass microbeads and carbon black, and mixing them with two-stage mixing. and vulcanization accelerator to ensure material uniformity and electrical insulation properties.
Significantly reduce the total weight of the sealing strip, improve electrical insulation performance, extend service life, conform to the trend of lightweight design, and improve automotive safety performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of elastomer rubber, and in particular to a method for preparing an EPDM insulating rubber sealing strip. Background Art
[0002] EPDM is a copolymer of ethylene, propylene and a small amount of non-conjugated dienes, called EPDM. The main chain of EPDM is composed of chemically stable saturated hydrocarbons, and only contains unsaturated double bonds in the side chains, so it is basically a saturated rubber. Since there are no polar substituents in the molecular structure and the cohesive energy between molecules is low, the molecular chain can maintain flexibility in a wide temperature range. It has excellent aging resistance such as ozone resistance, heat resistance, and weather resistance, and can be widely used in automotive parts, waterproof materials for construction, wire and cable sheaths, heat-resistant hoses, tapes, automotive seals and other fields.
[0003] After years of development, the rubber sealing strip industry has played an indispensable supporting role in the economy. EPDM materials have been widely used in various automotive systems due to their good comprehensive performance. With the rapid development of new energy vehicles, rubber sealing strips are also developing and upgrading in the direction of lightweight and insulation performance.
[0004] Traditional automotive sealing strips usually need to be filled with a large amount of inorganic materials such as kaolin and heavy calcium carbonate due to cost constraints. The density of these inorganic materials is generally 2.6g / cm 3 The rubber sealing strip composed of this material has a large specific gravity, and the weight of the sealing strip per unit volume is large. The amount of glue used has also increased significantly, resulting in an increase in production costs. According to the international general calculation method for automotive sealing strips, the average amount used for a single car is about 40 meters. The excessive specific gravity obviously does not meet the development needs of lightweight vehicles. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to provide a method for preparing a low-density, water-resistant EPDM insulating rubber sealing strip. The application of this new material can significantly reduce the total weight of the vehicle sealing strip, while improving the electrical insulation performance, and greatly improve the safety performance of new energy vehicles while pursuing lightweight design.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a low-density, water-resistant EPDM insulating rubber sealing strip, comprising the following steps: 1) Put EPDM rubber, reinforcing filler, nano-activated calcium carbonate, softening plasticizer and activator into an internal mixer and mix them to 120-130℃, then remove the hammer and clean them. Then put the hollow glass microsphere material into the internal mixer and mix them to 150-160℃ under the pressure of the hammer to discharge the rubber. Put the rubber on the open mixer and pound it for 180-240 seconds to produce sheets, obtain the first mixed rubber, and leave it for more than 24 hours. 2) Put 93-97% of the first mixed rubber and 3-7% of the vulcanization accelerator into an internal mixer for mixing, hammer mixing for 30-50 seconds and then clean up, continue hammer mixing for 40-60 seconds and then discharge the rubber, put the rubber on the open mixer for 180-240 seconds to produce sheets, and obtain a low-density, water-resistant EPDM insulating rubber sealing strip.
[0007] The present invention adopts a two-stage mixing method, and at the same time ensures that the interval between the first and second mixed rubbers is more than 24 hours. In the early stage of the first stage of mixing, EPDM rubber, nano-active calcium carbonate, reinforcing filler, plasticizer and activator are added together to ensure mixing uniformity, which is conducive to the dispersion of reinforcing filler (carbon black) and other materials, and ensures that the electrical insulation performance of the rubber material is consistent. The hollow glass microsphere material is added at 120-130°C, at which time the water contained in some materials has been completely evaporated and discharged, which can ensure that its activity is not affected. At the same time, the latter stage of addition can reduce its mixing time, and its hollow structure will not be damaged due to long-term mixing.
[0008] The EPDM rubber, reinforcing filler, nano-activated calcium carbonate, softening plasticizer, activator and hollow glass microsphere materials account for 30-40%, 15-20%, 10-30%, 10-20%, 2-5% and 10-20% of the total weight of the materials, respectively. The mixing process with this amount of materials is relatively stable, easy to operate and has low production cost. Among them, the new material of hollow glass microsphere is added. The hollow glass microsphere is a tiny hollow glass sphere, which is an inorganic non-metallic material with a typical particle size range of 10-180 microns and a bulk density of 0.1-0.25g / cm 3 , with the advantages of light weight, low thermal conductivity, sound insulation, high dispersion, good electrical insulation and thermal stability, it is a new type of lightweight material with wide applications and excellent performance developed in recent years. Based on the unique structure of hollow glass microspheres, it has excellent surface hydrophobicity, which can improve the sealing performance of vehicle and door and window sealing strips in rainy environments, and can also better avoid the corrosion of rainwater residue to rubber sealing strips, thereby increasing the service life of rubber sealing strips. At the same time, in order to improve the hydrophobic effect of the material of the present invention, nano-active calcium carbonate is added, which is a modified synthesis of stearate and calcium carbonate. Compared with ordinary calcium carbonate, nano-active calcium carbonate has better surface wettability, which can increase the interfacial compatibility with rubber polymers and achieve nanoscale dispersion, thereby improving the surface hydrophobicity of EPDM rubber sealing strip materials.
[0009] In addition, the EPDM rubber described in the present invention is Keltan 10675C of ARLANXEO. The reinforcing filler is carbon black N550. The present invention selects Keltan 10675C as the main material of EPDM rubber, which itself has the advantages of low density and high Mooney, and can be filled with a large amount of insulating materials. It also has the characteristics of high ethylene and high relative molecular mass. While being highly filled, the mechanical properties of the mixed rubber are good, the elasticity retention ability is strong, and it also has excellent processing characteristics, vulcanization characteristics and heat-resistant air aging performance. The addition of the reinforcing filler, Black Cat brand carbon black N550, can further improve the mechanical properties and low density characteristics of the rubber sealing strip, and also has good extrusion processability. DETAILED DESCRIPTION
[0010] The examples are as follows: 1. Weighing Each embodiment and control example was weighed according to the following Table 1.
[0011]
[0012] In Table 1, the EPDM rubber is Keltan 10675C from ARLANXEO. The reinforcing filler is Black Cat brand carbon black N550. The nano-active calcium carbonate is the Dongnan brand nano-active calcium carbonate. The hollow glass microspheres are hollow glass microspheres from Zhengzhou Shenglait Company. The softening plasticizer is the high flash point paraffin oil from Zhongrun Company. Ordinary calcium carbonate, activator, and vulcanization accelerator are common commercial products.
[0013] 2. Preparation method (production process) 1. Ingredients: According to the proportion table of each example, EPDM rubber, reinforcing filler, nano-activated calcium carbonate, softening plasticizer and activator are weighed respectively to form ingredient A, hollow glass microspheres are weighed to form ingredient B, and vulcanization accelerator is weighed to form ingredient C.
[0014] 1) First mixing: Put ingredient A into internal mixer and mix until the temperature reaches 120-130℃, then lift the hammer to clean, then put ingredient B into internal mixer, mix until the temperature reaches 150-160℃ and discharge the rubber; put the rubber on open mixer and pound for 180-240 seconds to produce sheets, obtain the first mixed rubber, and leave it for more than 24 hours; 2) Second mixing: The first mixed rubber and ingredient C are put into an internal mixer for mixing, and the mixture is hammered for 30-50 seconds and then cleaned. The mixture is hammered for 40-60 seconds and then the rubber is discharged. The rubber is pounded on an open mixer for 180-240 seconds to produce sheets, thereby obtaining a low-density, water-resistant EPDM insulating rubber sealing strip (i.e., the second mixed rubber, which is stored for more than 24 hours).
[0015] As described above, the present invention adopts a two-stage mixing method, while ensuring that the interval between the first and second mixed rubbers is more than 24 hours. At the beginning of the first stage of mixing, EPDM rubber, nano-activated calcium carbonate, reinforcing fillers, plasticizers and activators are added together to ensure mixing uniformity, facilitate the dispersion of materials such as nano-calcium carbonate, and ensure that the electrical insulation properties of the rubber material are consistent. The hollow glass microsphere material is added at 120-130°C, at which time the water contained in some materials has been completely evaporated and discharged, which can ensure that its activity is not affected; at the same time, the latter stage of addition can reduce the mixing time, and its hollow structure will not be damaged due to long-term mixing.
[0016] 3. Test results of rubber sealing strip materials 1. The test results of mechanical properties, density and insulation properties of Examples 1-5 and Comparative Examples 1-3 are shown in Table 2.
[0017]
[0018] 2. The test results of the water-resistant volume expansion change rate of Examples 1-5 and Comparative Examples 1-3 are shown in Table 3.
[0019]
[0020] It can be seen from Table 2 that the low-density, water-resistant EPDM rubber sealing strip obtained by the present invention has excellent mechanical properties, meets the relevant national standards for rubber sealing strips, and can better prevent cracking during assembly and use, thereby extending the service life. Moreover, the relative density of the rubber sealing strip material obtained by the present invention is lower than that of the traditional sealing strip material. Assuming that the length of the sealing strip of a vehicle is 40 meters, the weight can be reduced by 25-30% by using the rubber sealing strip material prepared by the present invention. The application of the new rubber sealing strip material on automobile sealing strips can significantly reduce the total weight of the vehicle sealing strips, which is in line with the trend of lightweight automobile design. At the same time, the present invention can significantly improve the electrical insulation performance of the rubber sealing strip, and under the current trend of automobile electrification, it can improve automobile safety and ensure personal safety. It can be seen from Table 3 that the water-resistant volume expansion change rate of the low-density, water-resistant EPDM rubber sealing strip obtained by the present invention is smaller than that of the traditional rubber sealing strip material, which can extend the service life and improve the sealing performance of the rubber sealing strip material.
Claims
1. A method for preparing a low-density, water-resistant EPDM insulating rubber sealing strip, characterized in that: The following steps are involved: 1) Put EPDM rubber, reinforcing filler, nano-active calcium carbonate, softening plasticizer and activator into an internal mixer and mix them to 120-130°C, then remove the hammer and clean them. Then put the hollow glass microsphere material into the internal mixer and mix them to 150-160°C by hammering to discharge the rubber. Put the rubber on the open mixer and pound it for 180-240 seconds to produce sheets, obtain the first mixed rubber, and leave it for more than 24 hours. 2) Put 93-97% of the first mixed rubber and 3-7% of the vulcanization accelerator into an internal mixer for mixing, hammer mixing for 30-50 seconds and then clean up, continue hammer mixing for 40-60 seconds and then discharge the rubber, put the rubber on an open mixer for 180-240 seconds to produce sheets, and obtain a low-density, water-resistant EPDM insulating rubber sealing strip.
2. The method for preparing the low-density, water-resistant EPDM insulating rubber sealing strip according to claim 1, characterized in that: The EPDM rubber, reinforcing filler, nano-active calcium carbonate, softening plasticizer, activator and hollow glass microsphere material account for 30-40%, 15-20%, 10-30%, 10-20%, 2-5% and 10-20% of the total weight of the materials respectively.
3. The method for preparing the low-density, water-resistant EPDM insulating rubber sealing strip according to claim 1 or 2, characterized in that: The EPDM rubber is Keltan 10675C from ARLANXEO.
4. The method for preparing the low-density, water-resistant EPDM insulating rubber sealing strip according to claim 1 or 2, characterized in that: The nano-active calcium carbonate is Southeast brand nano-active calcium carbonate.
5. The method for preparing the low-density, water-resistant EPDM insulating rubber sealing strip according to claim 2, characterized in that: The hollow glass microsphere material is hollow glass microsphere produced by Saint-Light Corporation.
6. The method for preparing the low-density, water-resistant EPDM insulating rubber sealing strip according to claim 1, characterized in that: The reinforcing filler is carbon black N550.
7. The method for preparing the low-density, water-resistant EPDM insulating rubber sealing strip according to claim 1, characterized in that: The softening plasticizer is high flash point paraffin oil.
Citation Information
Cited By
Rubber compound for lightweight EPDM (Ethylene-Propylene-Diene Monomer) sealing strip and preparation process thereof
CN121086412A